Inorganic copper nano pesticide as well as preparation method and application thereof
By using inorganic copper nanopesticides combined with copper hydroxide and copper oxychloride and nano-calcium carbonate, the problems of low utilization rate and environmental pollution of existing copper preparations are solved, and the effect of efficient prevention and treatment of crop diseases is achieved.
Patent Information
- Application Number
- CN202411018932.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-29
AI Technical Summary
Existing copper preparations have a low utilization rate of copper atoms and poor bactericidal effect when preventing and treating crop diseases. After use, copper remains in the soil and pollutes the environment.
Using copper hydroxide and/or copper oxychloride as the copper precursor, combined with nano-calcium carbonate as the carrier, inorganic copper nanopesticides are prepared through ultrasonic loading, aging, solvent removal, high-temperature calcination and grinding depolymerization to improve the utilization rate of copper. and prevention effects.
It significantly improves the control effect of inorganic copper nanopesticides, reduces the amount of copper and environmental pollution, improves the utilization rate of copper, and can effectively prevent and control bacterial and fungal diseases.
Smart Images

Figure BDA0004966593790000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pesticide bactericides, and in particular relates to an inorganic copper nanopesticide and a preparation method and application thereof. Background Art
[0002] Crops often encounter a variety of diseases such as bacteria, fungi, viruses and nematodes when growing, which poses a great risk to the growth, breeding, storage and transportation of crops. In addition to necessary agricultural measures, the use of fungicides containing fungicidal active compounds to prevent and control these diseases is essential.
[0003] Copper preparations are a kind of agricultural fungicide with a long history. Existing copper preparations mainly include Bordeaux mixture, copper hydroxide, copper oxide, copper sulfate, basic copper sulfate, copper oxychloride, etc. However, existing copper preparations generally have the problems of low copper atom utilization rate and poor bactericidal effect. In order to achieve the prevention and control effect, it is necessary to increase the dosage of copper preparations. Copper is a heavy metal. After use, the residue in the soil will cause environmental pollution, especially the impact on the aquatic ecosystem.
[0004] Therefore, there is an urgent need for an inorganic copper nanopesticide with good control effect, high utilization rate and low dosage to solve the above problems. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides an inorganic copper nanopesticide and a preparation method and application thereof.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides an inorganic copper nanopesticide, wherein the content of copper element in the inorganic copper nanopesticide is 5-30%; the inorganic copper nanopesticide is prepared by using copper hydroxide and / or copper oxychloride as copper precursor, nano calcium carbonate as carrier, water or ethanol as solvent, and undergoing ultrasonic loading, aging, solvent removal, high temperature calcination and grinding depolymerization.
[0008] Preferably, the particle size of the copper precursor is 10-30 nm; and the average pore size of the nano-calcium carbonate is 100-200 nm.
[0009] Preferably, the preparation method of the nano calcium carbonate comprises the following steps: mixing Ca(OH)2 and 1-butyl-3-methylimidazolium chloride, carrying out a high pressure reaction under a CO2 atmosphere, washing and drying to obtain the nano calcium carbonate.
[0010] Preferably, the mass ratio of Ca(OH)2 and 1-butyl-3-methylimidazolium chloride is 1:(1-2); the temperature of the high-pressure reaction is 50-60°C, the time is 10-15min, and the pressure is 15-20MPa.
[0011] Preferably, the invention further comprises auxiliary agents, which include suspending agents, dispersing agents and stabilizers; the amount of the suspending agent is 0.1-0.3% of the weight of the copper precursor, the amount of the dispersing agent is 0.03-0.06% of the weight of the copper precursor, and the amount of the stabilizer is 0.05-0.1% of the weight of the copper precursor.
[0012] The present invention provides a method for preparing the inorganic copper nanopesticide described in the above technical solution, comprising the following steps:
[0013] (1) mixing nano-calcium carbonate, a copper precursor and a solvent, performing ultrasonic treatment, stirring, aging, evaporating the solvent and ball milling to obtain nano-calcium carbonate loaded with a copper precursor;
[0014] (2) calcining and grinding the nano calcium carbonate loaded with copper precursor obtained in step (1) to depolymerize to obtain an inorganic copper nano pesticide precursor;
[0015] (3) The inorganic copper nanopesticide precursor obtained in step (2) and the auxiliary agent are uniformly mixed and granulated to obtain the inorganic copper nanopesticide.
[0016] Preferably, in step (1), the aging temperature is room temperature and the time is 5-10 hours.
[0017] Preferably, in step (2), the calcination includes low-temperature calcination and high-temperature calcination; the temperature of the low-temperature calcination is 200-300°C and the time is 1-3h; the temperature of the high-temperature calcination is 400-550°C and the time is 3-6h.
[0018] The present invention also provides the use of the inorganic copper nanopesticide described in the above technical solution in preventing and controlling bacterial diseases and fungal diseases of crops.
[0019] Preferably, the inorganic copper nanopesticide needs to be diluted to a concentration of 10-25% before use.
[0020] Compared with the prior art, the present invention has the following advantages and technical effects:
[0021] The invention uses a copper precursor, nano-calcium carbonate and a solvent as raw materials, and nano-copper in the prepared nano-pesticide plays a major prevention and control effect, can effectively prevent and control bacterial diseases and fungal diseases of crops, and by using nano-copper containing copper oxide, compared with a single copper preparation, can significantly improve the prevention and control effect and reduce the amount of inorganic copper nano-pesticide; nano-calcium carbonate is used to control the particle size of nano-copper and improve the dispersibility of inorganic copper nano-pesticide, thereby ensuring the prevention and control effect and improving the utilization rate.
[0022] The content of copper in the inorganic copper nanopesticide provided by the invention is only 5-30%, and when diluted to a concentration of 10-25% during use, it can still effectively prevent and treat bacterial diseases and fungal diseases of crops, with significant prevention and treatment effects, improved copper utilization, and reduced environmental pollution caused by copper residues. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.
[0025] The embodiment of the present invention provides an inorganic copper nanopesticide, wherein the content of copper element in the inorganic copper nanopesticide is 5-30%; the inorganic copper nanopesticide is prepared by using copper hydroxide and / or copper oxychloride as copper precursor, nano calcium carbonate as carrier, water or ethanol as solvent, and undergoing ultrasonic loading, aging, solvent removal, high temperature calcination and grinding depolymerization.
[0026] The present invention uses copper precursor, nano calcium carbonate and solvent as raw materials, and nano copper in the prepared nano pesticide plays a major preventive effect, which can effectively prevent and treat bacterial diseases and fungal diseases of crops. By using nano copper containing copper oxide, compared with a single copper preparation, the preventive effect can be significantly improved, and the amount of inorganic copper nano pesticide can be reduced; nano calcium carbonate is used to control the particle size of nano copper, and at the same time improve the dispersibility of inorganic copper nano pesticide, thereby ensuring the preventive effect and improving the utilization rate. In addition, the content of copper in the inorganic copper nano pesticide provided by the present invention is only 5-30%, and when diluted to a concentration of 10-25% during use, it can still effectively prevent and treat bacterial diseases and fungal diseases of crops, with significant preventive effect, improved copper utilization, and reduced environmental pollution caused by copper residues.
[0027] In a preferred embodiment, the particle size of the copper precursor is 10-30 nm. The present invention uses a copper precursor with a particle size in the above range and combines nano calcium carbonate with an average pore size of 100-200 nm as a carrier to increase the loading rate of nano copper, thereby increasing the utilization rate of copper and significantly improving the control effect of inorganic copper nano pesticides.
[0028] The nano calcium carbonate in the present invention is used to load the copper precursor. In a preferred embodiment, the average pore size of the nano calcium carbonate is 100-200nm. The present invention is beneficial to controlling the particle size of nano copper by controlling the average particle size of the nano calcium carbonate, and is beneficial to improving the dispersibility of the inorganic copper nano pesticide on the other hand, thereby ensuring the control effect and improving the utilization rate of the inorganic copper nano pesticide.
[0029] In a preferred embodiment, the preparation method of the nano calcium carbonate comprises the following steps: mixing Ca(OH)2 and 1-butyl-3-methylimidazolium chloride, reacting under high pressure in a CO2 atmosphere, washing and drying to obtain the nano calcium carbonate. The nano calcium carbonate prepared by the preparation method of the present invention has uniform particle size distribution and good dispersibility. It can be used as a carrier to evenly disperse the copper precursor, thereby obtaining an inorganic copper nano pesticide that can effectively prevent and treat bacterial and fungal diseases of crops.
[0030] In a preferred embodiment, the mass ratio of Ca(OH)2 and 1-butyl-3-methylimidazolium chloride is 1:(1-2); the temperature of the high-pressure reaction is 50-60°C, the time is 10-15min, and the pressure is 15-20MPa.
[0031] In a preferred embodiment, the inorganic copper nanopesticide further comprises an adjuvant. The adjuvant in the present invention can improve the dispersibility and stability of the inorganic copper nanopesticide, thereby improving the uniformity and adhesion of the pesticide on the surface of crops, thereby achieving the purpose of effectively preventing and controlling bacterial and fungal diseases of crops.
[0032] In a preferred embodiment, the auxiliary agent includes a suspending agent, a dispersing agent and a stabilizer; the suspending agent includes one or more of xanthan gum, sodium carboxymethyl cellulose, sodium alginate, and soybean oil; the dispersing agent includes one or more of sodium lignin sulfonate, alkylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether; the stabilizer includes one or more of 1,2-butanediol, glycerol, and polyethylene glycol.
[0033] In a preferred embodiment, the amount of the suspending agent is 0.1-0.3% by weight of the copper precursor, preferably 0.15-0.25%; the amount of the dispersant is 0.03-0.06% by weight of the copper precursor, preferably 0.03-0.05%; the amount of the stabilizer is 0.05-0.1% by weight of the copper precursor, preferably 0.05-0.08%.
[0034] In a preferred embodiment, the amount of the solvent used is 10-15 times the total mass of the copper precursor and the nano-calcium carbonate.
[0035] The present invention provides a method for preparing the inorganic copper nanopesticide described in the above technical solution, comprising the following steps:
[0036] (1) mixing nano-calcium carbonate, a copper precursor and a solvent, performing ultrasonic treatment, stirring, aging, evaporating the solvent and ball milling to obtain nano-calcium carbonate loaded with a copper precursor;
[0037] (2) calcining and grinding the nano calcium carbonate loaded with the copper precursor obtained in step (1) to depolymerize to obtain an inorganic copper nano pesticide precursor;
[0038] (3) The inorganic copper nanopesticide precursor obtained in step (2) and the auxiliary agent are uniformly mixed and granulated to obtain the inorganic copper nanopesticide.
[0039] In a preferred embodiment, in step (1), the copper precursor includes one or both of copper oxychloride and copper hydroxide. In the present invention, copper oxychloride and copper hydroxide are used as copper precursors, which will partially decompose during the subsequent calcination process to generate copper oxide, thereby obtaining nano copper containing copper oxide. By using nano copper containing copper oxide, compared with a single copper preparation, the control effect can be significantly improved and the amount of inorganic copper nano pesticide can be reduced.
[0040] In a preferred embodiment, in step (1), the power of the ultrasonic treatment is 40-60KHz and the time is 20-40min. The present invention promotes uniform dispersion of the nano-calcium carbonate and the copper precursor and increases the contact area by mixing the nano-calcium carbonate and the copper precursor in a solvent and then treating them with ultrasonic waves.
[0041] In a preferred embodiment, in step (1), the stirring speed is 500-800 rpm and the stirring time is 2-6 hours. The present invention promotes more copper precursors to enter the pores of nano-calcium carbonate by continuing to mix under stirring conditions for a certain period of time after ultrasonic treatment.
[0042] In a preferred embodiment, in step (1), the aging temperature is room temperature, the time is 5-10 hours, and the method is static aging. The present invention further promotes the adsorption and penetration of the copper precursor on the surface of the nano-calcium carbonate through aging, which helps to increase the loading rate of the copper precursor.
[0043] In a preferred embodiment, in step (1), the temperature of evaporating the solvent is the boiling point of the solvent, and the time is 20-50 minutes. The present invention helps to fix the copper precursor on the nano-calcium carbonate by evaporating the solvent at an appropriate temperature to form a solid or semi-solid.
[0044] In a preferred embodiment, in step (1), the ball milling speed is 100-150 r / min, the time is 20-40 min, the grinding balls are zirconia balls, and the ball-to-material ratio is 5:1-10:1. The present invention further refines the particles through ball milling to promote the uniform distribution of the copper precursor on the nano-calcium carbonate.
[0045] In a preferred embodiment, in step (2), the calcination includes low-temperature calcination and high-temperature calcination; the temperature of the low-temperature calcination is 200-300°C and the time is 1-3h; the temperature of the high-temperature calcination is 400-550°C and the time is 3-6h. The present invention decomposes the copper precursor loaded on the surface of the nano-calcium carbonate through calcination to generate copper oxide, while the copper precursor loaded inside the nano-calcium carbonate does not decompose or decomposes a small amount, thereby obtaining a nano-copper mixture containing copper oxide, thereby improving the control effect of inorganic copper nano-pesticides.
[0046] In a preferred embodiment, in step (2), the grinding and deagglomeration has a rotation speed of 300-500 r / min, a time of 30-60 min, the grinding balls are zirconia balls, and the ball-to-material ratio is 5:1-10:1. The present invention refines the particle size of the particles obtained after high-temperature calcination by grinding and deagglomeration.
[0047] In a preferred embodiment, in step (3), the uniform mixing method is grinding; the grinding speed is 100-150r / min, the time is 20-40min, the grinding balls are zirconia balls, and the ball-to-material ratio is 5:1-10:1.
[0048] The present invention also provides the use of the inorganic copper nanopesticide described in the above technical solution in preventing and controlling bacterial diseases and fungal diseases of crops.
[0049] In a preferred embodiment, the concentration of the inorganic copper nanopesticide is 15-25%, preferably 15-20%.
[0050] In a preferred embodiment, the crops include rice, sorghum, sunflower, peanut, citrus, tobacco, kiwi, litchi, mango, grape, and cucumber.
[0051] In a preferred embodiment, the bacterial diseases include bacterial leaf streak, bacterial leaf blight, bacterial bacterial wilt, bacterial spot, bacterial angular leaf spot, and canker; the fungal diseases include rice smut, brown star disease, anthracnose, downy blight, and downy mildew.
[0052] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.
[0053] Example 1
[0054] An inorganic copper nanopesticide, the raw materials include: copper oxychloride, nano calcium carbonate, water and auxiliary agent; the amount of copper oxychloride is weighed as 8% of the total amount of nano calcium carbonate and copper oxychloride, and the amount of water is 10 times the total amount of nano calcium carbonate and copper oxychloride.
[0055] The particle size of copper oxychloride is 15-25nm; the average pore size of nano calcium carbonate is 120nm; the auxiliary agents are sodium carboxymethyl cellulose, sodium lignin sulfonate and polyethylene glycol, the amount of sodium carboxymethyl cellulose is 0.15% of the weight of copper oxychloride, the amount of sodium lignin sulfonate is 0.05% of the weight of copper oxychloride, and the amount of polyethylene glycol is 0.08% of the weight of copper oxychloride.
[0056] The preparation method of nano calcium carbonate is as follows: Ca(OH)2 and 1-butyl-3-methylimidazolium chloride are mixed in a mass ratio of 1:1 and then put into an autoclave, the temperature of the autoclave is set to 60°C and the pressure is set to 15MPa, carbon dioxide is introduced at the same time, the reaction is carried out for 10 minutes, and nano calcium carbonate is obtained after washing and drying.
[0057] Preparation process:
[0058] (1) nano-calcium carbonate, copper oxychloride and water were mixed and ultrasonically treated at 45 kHz for 25 minutes, then stirred at a speed of 550 rpm for 3 hours, allowed to stand for aging at room temperature for 6 hours, then the solvent was evaporated at 100° C. for 35 minutes, and finally ball milled at a speed of 150 r / min for 25 minutes, with zirconium oxide balls and a ball-to-material ratio of 5:1, to obtain nano-calcium carbonate loaded with copper oxychloride;
[0059] (2) calcining the copper oxychloride-loaded nano-calcium carbonate obtained in step (1) at 250° C. for 2 h, then calcining at 500° C. for 4 h, and then grinding and depolymerizing at a speed of 450 r / min for 45 min, with zirconium oxide balls as the grinding balls and a ball-to-material ratio of 5:1, to obtain an inorganic copper nano-pesticide precursor;
[0060] (3) The inorganic copper nanopesticide precursor obtained in step (2), sodium carboxymethyl cellulose, sodium lignin sulfonate, and polyethylene glycol are placed in a ball mill, and ball milled at a speed of 130 r / min for 35 min to make them uniformly mixed, the grinding balls are zirconium oxide balls, and the ball-to-material ratio is 5:1, and then granulation is performed to obtain the inorganic copper nanopesticide.
[0061] Example 2
[0062] An inorganic copper nanopesticide, the raw materials of which include copper hydroxide, nano calcium carbonate, water and auxiliary agent; the amount of copper hydroxide is weighed as 5% of the total amount of nano calcium carbonate and copper hydroxide, and the amount of water is 10 times of the total amount of nano calcium carbonate and copper hydroxide.
[0063] The particle size of copper hydroxide is 10-20nm; the average pore size of nano calcium carbonate is 150nm; the auxiliary agents are sodium alginate, fatty alcohol polyoxyethylene ether and glycerol; the amount of sodium alginate is 0.2% of the weight of copper hydroxide, the amount of fatty alcohol polyoxyethylene ether is 0.03% of the weight of copper hydroxide, and the amount of glycerol is 0.06% of the weight of copper hydroxide.
[0064] The preparation method of nano calcium carbonate is as follows: Ca(OH)2 and 1-butyl-3-methylimidazolium chloride are mixed in a mass ratio of 1:1 and then put into an autoclave, the temperature of the autoclave is set to 55°C and the pressure is set to 15MPa, carbon dioxide is introduced at the same time, the reaction is carried out for 15 minutes, and nano calcium carbonate is obtained after washing and drying.
[0065] Preparation process:
[0066] (1) After mixing nano-calcium carbonate, copper hydroxide and water, ultrasonic treatment was performed at 45KHz for 35 minutes, and then stirred at a speed of 600rpm for 3 hours, and aged at room temperature for 8 hours, and then the solvent was evaporated at 100°C for 35 minutes, and finally ball milled at a speed of 120r / min for 35 minutes, the grinding balls were zirconia balls, and the ball-to-material ratio was 6:1, to obtain nano-calcium carbonate loaded with copper hydroxide;
[0067] (2) calcining the copper hydroxide-loaded nano-calcium carbonate obtained in step (1) at 280° C. for 1 h, then calcining at 400° C. for 3 h, and then grinding and depolymerizing at a speed of 450 r / min for 45 min, with zirconium oxide balls as the grinding balls and a ball-to-material ratio of 6:1, to obtain an inorganic copper nano-pesticide precursor;
[0068] (3) The inorganic copper nanopesticide precursor obtained in step (2) and sodium alginate, fatty alcohol polyoxyethylene ether, and glycerol are placed in a ball mill, and ball milled for 35 minutes at a speed of 130 r / min to make them uniformly mixed, the grinding balls are zirconia balls, and the ball-to-material ratio is 6:1, and then granulation is performed to obtain the inorganic copper nanopesticide.
[0069] Example 3
[0070] An inorganic copper nanopesticide is composed of the following raw materials in parts by weight: the raw materials include: a copper precursor (the molar ratio of copper hydroxide to copper oxychloride is 1:1), nano calcium carbonate, water and an auxiliary agent; wherein the amount of copper hydroxide and copper oxychloride is weighed so that the copper element accounts for 15% of the total amount of nano calcium carbonate+copper hydroxide+copper oxychloride, and the amount of water is 10 times the total amount of nano calcium carbonate+copper hydroxide+copper oxychloride.
[0071] The particle size of the copper precursor is 12-20nm; the average pore size of nano calcium carbonate is 180nm; the additives are soybean oil, alkylphenol polyoxyethylene ether and 1,2-butanediol, the amount of soybean oil is 0.3% of the weight of the copper precursor, the amount of alkylphenol polyoxyethylene ether is 0.5% of the weight of the copper precursor, and the amount of 1,2-butanediol is 0.08% of the weight of the copper precursor.
[0072] The preparation method of nano calcium carbonate is as follows: Ca(OH)2 and 1-butyl-3-methylimidazolium chloride are mixed in a mass ratio of 1:1 and then put into an autoclave, the temperature of the autoclave is set to 50°C and the pressure is set to 15MPa, carbon dioxide is introduced at the same time, the reaction is carried out for 10 minutes, and nano calcium carbonate is obtained after washing and drying.
[0073] Preparation process:
[0074] (1) nano-calcium carbonate, copper oxychloride, copper hydroxide and ethanol were mixed and ultrasonically treated at 50 kHz for 20 minutes, then stirred at a speed of 800 rpm for 2 hours, left to stand for aging at room temperature for 6 hours, then the solvent was evaporated at 80° C. for 40 minutes, and finally ball milled at a speed of 150 r / min for 25 minutes, with zirconium oxide balls and a ball-to-material ratio of 5:1, to obtain nano-calcium carbonate loaded with a copper precursor;
[0075] (2) calcining the nano calcium carbonate loaded with copper precursor obtained in step (1) at 220° C. for 3 h, then calcining at 450° C. for 5 h, and then grinding and depolymerizing at a speed of 380 r / min for 60 min, with zirconium oxide balls as the grinding balls and a ball-to-material ratio of 5:1, to obtain an inorganic copper nano pesticide precursor;
[0076] (3) The inorganic copper nanopesticide precursor obtained in step (2), soybean oil, alkylphenol polyoxyethylene ether, and 1,2-butanediol are placed in a ball mill, and ball milled for 35 minutes at a speed of 130 r / min to make them uniformly mixed, the grinding balls are zirconium oxide balls, and the ball-to-material ratio is 5:1, and then granulation is performed to obtain the inorganic copper nanopesticide.
[0077] Example 4
[0078] An inorganic copper nanopesticide is composed of the following raw materials in parts by weight: the raw materials include: a copper precursor (the molar ratio of copper hydroxide to copper oxychloride is 1:1), nano calcium carbonate, water and an auxiliary agent; wherein the amount of copper hydroxide and copper oxychloride is weighed such that the copper element accounts for 10% of the total amount of nano calcium carbonate+copper hydroxide+copper oxychloride, and the amount of water is 10 times the total amount of nano calcium carbonate+copper hydroxide+copper oxychloride.
[0079] The particle size of the copper precursor is 15-30nm; the average pore size of the nano calcium carbonate is 180nm; the additives are sodium carboxymethyl cellulose, sodium lignin sulfonate and polyethylene glycol; the amount of sodium carboxymethyl cellulose is 0.3% of the weight of the copper precursor, the amount of sodium lignin sulfonate is 0.06% of the weight of the copper precursor, and the amount of polyethylene glycol is 0.1% of the weight of the copper precursor.
[0080] The preparation method of nano calcium carbonate is as follows: Ca(OH)2 and 1-butyl-3-methylimidazolium chloride are mixed in a mass ratio of 1:1 and then put into an autoclave, the temperature of the autoclave is set to 50°C and the pressure is set to 15MPa, carbon dioxide is introduced at the same time, the reaction is carried out for 10 minutes, and nano calcium carbonate is obtained after washing and drying.
[0081] Preparation process:
[0082] (1) nano-calcium carbonate, copper oxychloride, copper hydroxide and ethanol were mixed and ultrasonically treated at 45 kHz for 25 minutes, then stirred at a speed of 550 rpm for 3 hours, left to stand for aging at room temperature for 6 hours, then the solvent was evaporated at 80° C. for 35 minutes, and finally ball milled at a speed of 150 r / min for 25 minutes, with the grinding balls being zirconium oxide balls and the ball-to-material ratio being 5:1, to obtain nano-calcium carbonate loaded with a copper precursor;
[0083] (2) calcining the nano calcium carbonate loaded with copper precursor obtained in step (1) at 300° C. for 2 h, then calcining at 500° C. for 4 h, and then grinding and depolymerizing at a speed of 450 r / min for 45 min, with zirconium oxide balls as the grinding balls and a ball-to-material ratio of 5:1, to obtain an inorganic copper nano pesticide precursor;
[0084] (3) The inorganic copper nanopesticide precursor obtained in step (2), sodium carboxymethyl cellulose, sodium lignin sulfonate, and polyethylene glycol are placed in a ball mill, and ball milled at a speed of 130 r / min for 35 min to make them uniformly mixed, the grinding balls are zirconium oxide balls, and the ball-to-material ratio is 5:1, and then granulation is performed to obtain the inorganic copper nanopesticide.
[0085] Comparative Example 1
[0086] The difference from Example 1 is that the copper precursor is copper oxide.
[0087] Comparative Example 2
[0088] The difference from Example 1 is that the copper precursor is copper oxychloride, the calcination step is replaced by drying at 100° C., and the nano copper in the obtained inorganic copper nano pesticide is copper oxychloride.
[0089] Comparative Example 3
[0090] The difference from Example 1 is that the copper precursor is copper hydroxide, the calcination step is replaced by drying at 100° C., and the nano-copper in the obtained inorganic copper nano-pesticide is copper hydroxide.
[0091] Comparative Example 4
[0092] The difference from Example 1 is that in step (2), the calcination is first performed at 280° C. for 1 h and then at 1000° C. for 3 h.
[0093] Comparative Example 5
[0094] The difference from Example 1 is that in step (2), the nano calcium carbonate loaded with copper hydroxide obtained in step (1) is calcined at 400° C. for 3 h.
[0095] Comparative Example 6
[0096] The difference from Example 1 is that the preparation method of nano calcium carbonate is: under stirring conditions, 0.2 mol / L CaCl2 solution and 0.1 mol / L sodium dodecyl sulfate solution are mixed in a volume ratio of 1:1 to obtain a mixed solution; then, a 0.2 mol / L Na2CO3 solution of an equal volume to the above mixed solution is added, and the precipitate is collected by centrifugation, washed three times with deionized water and anhydrous ethanol respectively, dried in an oven at 60°C, and then calcined at 350°C for 3h to obtain nano calcium carbonate.
[0097] Field trials
[0098] Control target: Rice bacterial leaf streak; Crops: Rice;
[0099] Ten test plots were set up to conduct field control experiments on bacterial leaf streak of rice. Spraying was used as the pesticide application method with a pesticide concentration of 10% and a dosage of 50 g / mu. The first application was made at the peak of rice tillering and the second application was made 7 days later, for a total of two applications. The disease index was measured 3, 7, 14, 20 and 30 days after application, and the efficacy was calculated.
[0100] Table 1 Control effect of Examples 1-4 and Comparative Examples 1-6
[0101]
[0102] It can be seen from Table 1 that the inorganic copper nanopesticide provided by the present invention has a copper content of 15%, is diluted to a concentration of 10% when used, and has a dosage of 50 g / mu. The 3-day protection effect can reach 93.64%, the 7-day protection effect can reach 89.71%, the 14-day protection effect can reach 87.04%, the 20-day protection effect can reach 84.23%, and the 30-day protection effect can reach 81.91%. This shows that the inorganic copper nanopesticide provided by the present invention can effectively prevent and control bacterial diseases of crops at a lower concentration, improve the utilization rate of copper, and have excellent prevention and control effects compared with single copper oxide, copper oxychloride or copper hydroxide. Comparative Example 1 only uses copper oxide as the copper precursor, and the 7-day protection effect decreases by 14.01% compared with Example 1; Comparative Examples 2 and 3 replace the calcination step with drying, and the 7-day protection effect decreases by 13.23% and 11.92% respectively compared with Example 1; Comparative Example 4 increases the temperature of high-temperature calcination, and the 7-day protection effect decreases by 14.24% compared with Example 1; Comparative Example 5 omits the low-temperature calcination step, and the 7-day protection effect decreases by 9.15% compared with Example 1; Comparative Example 6 changes the preparation method of nano calcium carbonate, and the 7-day protection effect decreases by 9.9% compared with Example 1.
[0103] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. An inorganic copper nanopesticide, characterized in that: The content of copper element in the inorganic copper nanopesticide is 5-30%; the inorganic copper nanopesticide is prepared by using copper hydroxide and / or copper oxychloride as copper precursor, nano calcium carbonate as carrier, water or ethanol as solvent, and undergoing ultrasonic loading, aging, solvent removal, high temperature calcination and grinding depolymerization.
2. The inorganic copper nanopesticide according to claim 1, characterized in that: The particle size of the copper precursor is 10-30nm; the average pore size of the nano calcium carbonate is 100-200nm.
3. The inorganic copper nanopesticide according to claim 1, characterized in that: The preparation method of the nano calcium carbonate comprises the following steps: mixing Ca(OH)2 and 1-butyl-3-methylimidazolium chloride, carrying out high pressure reaction under CO2 atmosphere, washing and drying to obtain the nano calcium carbonate.
4. The inorganic copper nanopesticide according to claim 3, characterized in that: The mass ratio of Ca(OH)2 and 1-butyl-3-methylimidazolium chloride is 1:(1-2); the temperature of the high-pressure reaction is 50-60°C, the time is 10-15min, and the pressure is 15-20MPa.
5. The inorganic copper nanopesticide according to claim 1, characterized in that: The invention also comprises auxiliary agents, which include suspending agent, dispersing agent and stabilizer; the dosage of the suspending agent is 0.1-0.3% of the weight of the copper precursor, the dosage of the dispersing agent is 0.03-0.06% of the weight of the copper precursor, and the dosage of the stabilizer is 0.05-0.1% of the weight of the copper precursor.
6. The method for preparing the inorganic copper nanopesticide according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing nano-calcium carbonate, a copper precursor and a solvent, performing ultrasonic treatment, stirring, aging, evaporating the solvent and ball milling to obtain nano-calcium carbonate loaded with a copper precursor; (2) calcining and grinding the nano calcium carbonate loaded with copper precursor obtained in step (1) to depolymerize to obtain an inorganic copper nano pesticide precursor; (3) The inorganic copper nanopesticide precursor obtained in step (2) and the auxiliary agent are uniformly mixed and granulated to obtain the inorganic copper nanopesticide.
7. The preparation method according to claim 6, characterized in that: In step (1), the aging temperature is room temperature and the aging time is 5-10 hours.
8. The preparation method according to claim 6, characterized in that: In step (2), the calcination includes low-temperature calcination and high-temperature calcination; the temperature of the low-temperature calcination is 200-300°C and the time is 1-3h; the temperature of the high-temperature calcination is 400-550°C and the time is 3-6h.
9. Use of the inorganic copper nanopesticide according to any one of claims 1 to 5 in preventing and controlling bacterial diseases and fungal diseases of crops.
10. The use according to claim 9, characterized in that: The inorganic copper nanopesticide is diluted to a concentration of 10-25% when used.