A catalyst and its preparation method and application
By using carbon material catalysts co-doped with iron and nitrogen, the problems of low selectivity and low conversion in the ethylbenzene peroxidation method are solved, efficient catalytic performance improvement and by-product reduction are achieved, and wastewater treatment problems are solved .
Patent Information
- Application Number
- CN202411321660.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-23
AI Technical Summary
The existing ethylbenzene peroxidation method has low selectivity in the production of ethylbenzene hydrogen peroxide, low conversion rate and many by-products, resulting in wastewater treatment difficulties.
Carbon materials co-doped with iron and nitrogen are used as catalysts, and they exist through Fe-N4 coordination form to form a porous structure, improve catalytic performance, and prepare catalysts by chemical vapor deposition method to optimize specific surface area and pore volume.
The catalytic performance of ethylbenzene hydrogen peroxide is significantly improved, the raw material conversion rate and reaction selectivity are improved, and the generation of by-products is reduced.
Smart Images

Figure CN118847186B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of catalytic materials, and specifically relates to a catalyst and a preparation method and application thereof. Background Art
[0002] Propylene oxide (PO) is an important chemical raw material, which is mainly used to produce polyether polyols, propylene glycol, dimethyl carbonate, propylene glycol ether, etc. It has a wide range of applications and a large market demand. At present, the main methods for industrial production of propylene oxide are the chlorohydrin method, the co-oxidation method (including isobutane co-oxidation method, ethylbenzene peroxidation method and isobutylene peroxidation method) and the direct oxidation method of hydrogen peroxide (HPPO). Among them, the chlorohydrin method is limited in its promotion and application due to the generation of a large amount of wastewater and waste residue, environmental pollution, and serious corrosion of equipment. The HPPO method also has certain defects due to the high cost of raw materials and low device profits.
[0003] In the co-oxidation method, the ethylbenzene peroxidation method (PO / SM) can produce styrene (SM) while producing propylene oxide products. Due to its low production cost, low environmental pollution, and the ability to produce by-products to increase revenue, this method is currently widely used in the production of propylene oxide. The PO / SM process uses ethylbenzene hydroperoxide (EBHP) to oxidize propylene to produce propylene oxide and phenylethyl alcohol (PMA). The production of ethylbenzene hydroperoxide is mainly based on ethylbenzene as a raw material and air as an oxidant under high temperature and high pressure conditions. The conversion rate of ethylbenzene is between 6% and 7%, and the selectivity of EBHP is about 86%. Due to the low selectivity of the reaction, more phenylethyl alcohol, acetophenone and small molecular acid substances are generated. The subsequent process needs to add a large amount of alkali solution to wash out the impurities in EBHP, resulting in the production of a large amount of high-salt, high-COD wastewater in the process, and wastewater treatment is a difficult problem in the industry.
[0004] Therefore, it is necessary to find a catalyst with excellent catalytic performance to improve the product selectivity in the process of preparing ethylbenzene hydroperoxide by ethylbenzene peroxidation and reduce the generation of by-products, thereby solving the above-mentioned process problems of PO / SM. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present application is to overcome the defects of poor product selectivity and low raw material conversion rate in the process of preparing ethylbenzene hydrogen peroxide by ethylbenzene peroxidation in the prior art, thereby providing a catalyst and its preparation method and application.
[0006] To this end, this application provides the following technical solutions:
[0007] The present application provides a catalyst, which has a hollow structure and comprises a carbon material co-doped with iron and nitrogen.
[0008] Among them, the iron element exists in the form of Fe-N4 coordination.
[0009] In some optional embodiments, based on the mass of the catalyst, iron accounts for 0.06%-0.10%, and nitrogen accounts for 10.0%-12.7%. Typically, but not limited to, based on the mass of the catalyst, iron accounts for 0.06%, 0.07%, 0.08%, 0.083%, 0.085%, 0.09%, 0.092%, 0.095%, 0.098%, 0.10%, or in the range of any of the above values; nitrogen accounts for 10%, 11.0%, 11.3%, 11.5%, 11.7%, 11.9%, 12.0%, 12.3%, 12.5%, 12.7%, or in the range of any of the above values.
[0010] In the present application, the contents of iron and nitrogen in the catalyst are limited to the above ranges, and a higher content of single-atom iron dispersion and coordination with nitrogen can form excellent Fe-N4 coordinated catalytic active sites.
[0011] In some optional embodiments, the specific surface area of the catalyst is 400 m 2 / g-463.9m 2 / g, and the total pore volume is 0.96cm 3 / g-1.69cm 3 / g, and the mesopore volume is 0.65cm 3 / g-1.05cm 3 Typically, but not limiting, the specific surface area of the catalyst is 400m 2 / g,410m 2 / g, 420m 2 / g,425m 2 / g,430m 2 / g,440m 2 / g,450m 2 / g,460m 2 / g,470m 2 / g, or within the range of any of the above values; the total pore volume is 0.96cm 3 / g,1.00cm 3 / g, 1.10cm 3 / g, 1.20cm 3 / g, 1.25cm 3 / g,1.30cm 3 / g,1.46cm 3 / g,1.52cm 3 / g,1.60cm 3 / g,1.69cm3 / g, or within the range of any of the above values; the mesopore volume is 0.65cm 3 / g, and the mesopore volume is 0.65cm 3 / g,0.70cm 3 / g, 0.75cm 3 / g,0.80cm 3 / g,0.84cm 3 / g,0.92cm 3 / g, 0.97cm 3 / g, 1.01cm 3 / g,1.05cm 3 / g, or any of the above values within the range.
[0012] In the present application, the specific surface area, total pore volume and mesopore volume of the catalyst are limited to the above ranges. A higher specific surface area of the catalyst and more mesopores are helpful to the mass transfer process of the reaction.
[0013] The present application also provides a method for preparing a catalyst, comprising the following steps:
[0014] S1, mixing a carbon and nitrogen source with an iron source to obtain a mixed material, and depositing the mixed material onto nano-calcium carbonate by chemical vapor deposition;
[0015] S2, removing the nano calcium carbonate by acid treatment to obtain the catalyst.
[0016] In the present application, the purpose of the acid treatment is to etch away the calcium carbonate used as a template to form a hollow structure. The specific operation is conventional in the field. For example, the treatment can be performed by soaking in hydrochloric acid with a concentration of 1 mol / L-2 mol / L.
[0017] In some optional embodiments, in step S1, the molar ratio of the carbon-nitrogen source to the iron source is 60-800:1; typically, but not limiting, the molar ratio of the carbon-nitrogen source to the iron source is 60:1, 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, or within the range of any of the above values; the present application ensures that iron is anchored on the C / N substrate in a single-atom dispersed form by limiting the molar ratio of the carbon-nitrogen source to the iron source.
[0018] And / or, the average particle size of the nano calcium carbonate is 100nm-150nm; typically, but not limitedly, the average particle size of the nano calcium carbonate is 100nm, 105nm, 110nm, 120nm, 130nm, 135nm, 140nm, 150nm, or within the range of any of the above values. The present application ensures better mass transfer effect during the catalytic reaction by limiting the average particle size of the nano calcium carbonate.
[0019] In some optional embodiments, the temperature of the chemical vapor deposition is 800°C-1000°C; typically, but not limitedly, the temperature of the chemical vapor deposition is 800°C, 850°C, 900°C, 950°C, 1000°C, or within the range of any of the above values;
[0020] And / or, the heating rate of the chemical vapor deposition is 10°C / min-30°C / min; typically, but not limitedly, the heating rate of the chemical vapor deposition is 10°C / min, 15°C / min, 20°C / min, 25°C / min, 30°C / min, or within the range of any of the above values;
[0021] And / or, the chemical vapor deposition time is 10 min-60 min; typically, but not limitedly, the chemical vapor deposition time is 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, or within the range of any of the above values;
[0022] And / or, the gas rate of the chemical vapor deposition is 80sccm-200sccm; typically, but not limitedly, the gas rate of the chemical vapor deposition is 80sccm, 85sccm, 90sccm, 95sccm, 100sccm, 130sccm, 150sccm, 180sccm, 200sccm, or within a range consisting of any of the above values.
[0023] In some optional embodiments, the carbon and nitrogen source includes at least one of organic substances containing both carbon and nitrogen elements;
[0024] And / or, the iron source comprises at least one of soluble iron sources.
[0025] In some optional embodiments, the carbon and nitrogen source includes at least one of pyrridine, pyrrole, and ethylenediamine;
[0026] And / or, the iron source includes at least one of ferric chloride, ferric acetylacetonate, ferric acetate, and ferric sulfate.
[0027] The present invention also provides an application of the catalyst or the catalyst prepared by the preparation method in ethylbenzene peroxidation reaction.
[0028] In some optional embodiments, the reaction temperature of the ethylbenzene peroxidation reaction is 125°C-145°C, and the reaction pressure is 0.1MPaG-0.3MPaG. Typically, but not limited to, the reaction temperature of the ethylbenzene peroxidation reaction is 125°C, 130°C, 135°C, 140°C, 145°C, or within the range of any of the above values; the reaction pressure is 0.1MPaG, 0.15MPaG, 0.2MPaG, 0.25MPaG, 0.3MPaG, or within the range of any of the above values.
[0029] In the present application, the specific application method of the above catalyst in ethylbenzene peroxidation is conventional in the field, for example, it may include: loading the catalyst into a fixed bed reactor, allowing ethylbenzene and air to flow through the reactor to undergo peroxidation reaction to obtain ethylbenzene hydrogen peroxide.
[0030] In some optional embodiments, the space velocity of ethylbenzene is 1×10 -3 h -1 ~1×10 -1 h -1 .
[0031] In some optional embodiments, air is used as the oxidant, and the mass ratio of air to ethylbenzene is 0.001-0.1.
[0032] The technical solution of this application has the following advantages:
[0033] The catalyst provided by the present application is a hollow structure, and the composition of the catalyst includes a carbon material co-doped with iron and nitrogen, wherein the iron is present in the form of Fe-N4 coordination. The catalyst is a porous structure catalyst having active sites in the form of Fe-N4 coordination, and the introduction of active sites in the form of Fe-N4 coordination can effectively improve the catalytic performance of the catalyst for the reaction of ethylbenzene peroxidation to prepare ethylbenzene hydrogen peroxide, effectively improve the raw material conversion rate and reaction selectivity, and reduce the generation of by-products.
[0034] The catalyst provided in the present application can further improve the raw material conversion rate and reaction selectivity of the catalyst by limiting the element content, specific surface area and pore volume.
[0035] The preparation method of the catalyst provided in the present application comprises the following steps: S1, mixing a carbon and nitrogen source with an iron source to obtain a mixed material, and depositing the mixed material on nano-calcium carbonate by chemical vapor deposition; S2, removing the nano-calcium carbonate by acid treatment to obtain the catalyst. The catalyst prepared by chemical vapor deposition in the present application has an excellent mesoporous structure and a large specific surface area, which is beneficial to the mass transfer process in the reaction and helps to improve the catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0037] Figure 1 is a SEM electron microscope image of the catalyst provided in Example 2 of the present application;
[0038] Figure 2 This is the XPS spectrum of the nitrogen element in the catalyst provided in Example 2 of the present application. DETAILED DESCRIPTION
[0039] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0040] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0041] Example 1
[0042] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0043] (1) Add 0.146 g of ferric acetylacetonate into 20 mL of pyridine solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the pyridine solution;
[0044] (2) adding the fully mixed pyridine-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0045] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0046] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0047] (5) After the temperature in step (4) is raised to 900° C., the pyridine-iron acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 minutes to allow the precursor to be deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0048] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0049] Example 2
[0050] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0051] (1) Add 0.439 g of ferric acetylacetonate into 20 mL of pyridine solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the pyridine solution;
[0052] (2) adding the fully mixed pyridine-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0053] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0054] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0055] (5) After the temperature in step (4) is raised to 900° C., the pyridine-iron acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 minutes to allow the precursor to be deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0056] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0057] Figure 1 : is a SEM image of the catalyst obtained in this example. It can be seen from the figure that the catalyst is a hollow spherical structure, and the particle size diameter is distributed between 100-200 nm; Figure 2 It is the XPS spectrum of nitrogen element in the catalyst obtained in this embodiment. It can be seen from the figure that the four main nitrogen peaks correspond to pyridinic nitrogen, pyrrolic nitrogen, graphitic nitrogen and oxidized nitrogen, respectively. Different coordination forms with iron and carbon constitute different nitrogen species. The high content of nitrogen coordination ensures that the catalyst has good catalytic activity. The SEM images and XPS spectra of the catalysts provided in other embodiments are similar to those in this embodiment and are not shown one by one.
[0058] Example 3
[0059] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0060] (1) Add 1.462 g of ferric acetylacetonate into 20 mL of pyridine solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the pyridine solution;
[0061] (2) adding the fully mixed pyridine-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0062] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0063] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0064] (5) After the temperature in step (4) is raised to 900° C., the pyridine-iron acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 minutes to allow the precursor to be deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0065] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0066] Example 4
[0067] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0068] (1) Add 0.439 g of ferric acetylacetonate into 20 mL of pyridine solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the pyridine solution;
[0069] (2) adding the fully mixed pyridine-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0070] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0071] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 800°C at a heating rate of 30°C / min;
[0072] (5) After the temperature in step (4) is raised to 800° C., the pyridine-iron acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 minutes, so that the precursor is deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0073] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 h to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain catalyst 4.
[0074] Example 5
[0075] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0076] (1) Add 0.439 g of ferric acetylacetonate into 20 mL of pyridine solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the pyridine solution;
[0077] (2) adding the fully mixed pyridine-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0078] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0079] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 1000°C at a heating rate of 30°C / min;
[0080] (5) After the temperature in step (4) is raised to 1000° C., the pyridine-iron acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 minutes to allow the precursor to be deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0081] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0082] Example 6
[0083] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0084] (1) Add 0.146 g of ferric chloride to 20 mL of pyrrole solution, and stir the solution at room temperature for two hours to allow the ferric chloride to fully dissolve in the pyrrole solution;
[0085] (2) adding the fully mixed pyrrole-ferric chloride solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0086] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 100 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0087] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0088] (5) After the temperature in step (4) is raised to 900° C., the pyrrole-ferric chloride solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 100.0 sccm for 40 minutes, so that the precursor is deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0089] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0090] Example 7
[0091] This embodiment provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0092] (1) Add 0.234 g of ferric chloride to 20 mL of pyrrole solution, and stir the solution at room temperature for two hours to allow the ferric chloride to fully dissolve in the pyrrole solution;
[0093] (2) adding the fully mixed pyrrole-ferric chloride solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0094] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 130 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0095] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 920°C at a heating rate of 30°C / min;
[0096] (5) After the temperature in step (4) is raised to 920° C., the pyrrole-ferric chloride solution is introduced into the tube furnace through a bubbling system, and the gas rate is adjusted to 150.0 sccm for 30 min to deposit the precursor on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0097] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0098] Comparative Example 1
[0099] This comparative example provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0100] (1) No iron source was added, and only pyridine solution was added to the round-bottom flask of the chemical vapor deposition system (CVD) as a precursor;
[0101] (2) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size of 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0102] (3) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0103] (4) After the temperature in step (3) is raised to 900° C., the pyridine solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 min, so that the precursor is deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0104] (5) The powder sample obtained in step (4) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 h to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a comparative catalyst.
[0105] Comparative Example 2
[0106] This comparative example provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0107] (1) Weigh 14.8 g of ammonium chloride and dissolve it in 20 g of n-hexane solution as a carbon and nitrogen source precursor.
[0108] (2) Add 0.439 g of ferric acetylacetonate into 20 mL of n-hexane solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the pyridine solution;
[0109] (3) adding the fully mixed n-hexane-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0110] (4) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0111] (5) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0112] (6) After the temperature in step (4) is raised to 900° C., the n-hexane-ferric acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 min to deposit the precursor on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0113] (7) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 h to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0114] Comparative Example 3
[0115] This comparative example provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0116] (1) Pyridine solution was added into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0117] (2) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0118] (3) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0119] (4) After the temperature in step (3) is raised to 900° C., the pyridine solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 min, so that the precursor is deposited on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0120] (5) placing the powder sample obtained in step (4) into a 1M hydrochloric acid solution and stirring at 80°C for 12 hours to remove the nano-calcium carbonate template, and then washing, filtering, and drying the sample to obtain a carbonitride substrate;
[0121] (6) Weigh 0.439 g of ferric acetylacetonate, mix thoroughly with the carbonitride substrate prepared in step (5), and evenly place the mixture into a quartz boat. Place the quartz boat into a muffle furnace and heat to 900° C. for 20 min. Then cool the mixture naturally to room temperature and take it out to obtain a catalyst.
[0122] Comparative Example 4
[0123] This comparative example provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0124] (1) Add 0.439 g of ferric acetylacetonate into 20 mL of n-hexane solution, and stir the solution at room temperature for two hours to allow the ferric acetylacetonate to fully dissolve in the n-hexane solution;
[0125] (2) adding the fully mixed n-hexane-ferric acetylacetonate solution prepared in step (1) into a round-bottom flask of a chemical vapor deposition (CVD) system as a precursor;
[0126] (3) Use a balance to weigh 2 g of nano-calcium carbonate template (average particle size 150 nm) and evenly place it in a quartz boat, then place the quartz boat in the center of the tube furnace of the chemical vapor deposition system (CVD) close to the thermocouple temperature measurement point;
[0127] (4) Nitrogen was introduced into the CVD system as a protective gas, and the temperature was set to increase the temperature of the tube furnace to 900°C at a heating rate of 30°C / min;
[0128] (5) After the temperature in step (4) is raised to 900° C., the n-hexane-ferric acetylacetonate solution is introduced into the tube furnace through a bubbling system, and the gas speed is adjusted to 200.0 sccm for 20 min to deposit the precursor on the nano-calcium carbonate template at high temperature, and then naturally cooled to room temperature in a nitrogen flow;
[0129] (6) The powder sample obtained in step (5) was placed in a 1M hydrochloric acid solution and stirred at 80°C for 12 hours to remove the nano-calcium carbonate template. After washing and filtering, the sample was dried to obtain a catalyst.
[0130] Comparative Example 5
[0131] This comparative example provides a catalyst, and its preparation method and specific operating parameters are as follows:
[0132] (1) Weigh 0.29 g of ferric chloride and 10 g of dicyandiamide and dissolve them in 100 ml of deionized water;
[0133] (2) Place the solution prepared in step (1) in an oil bath and heat to 110°C, fully stir and heat until the water evaporates to obtain a light yellow solid powder;
[0134] (3) evenly placing the powder prepared in step (2) in a quartz boat, and placing the quartz boat in a tube furnace;
[0135] (4) Nitrogen was introduced into the muffle furnace as a protective gas, and the tube furnace was heated to 650°C at a heating rate of 5°C / min. After maintaining the temperature for 3 h under a nitrogen atmosphere, the temperature was naturally cooled and the sample was taken out to obtain the catalyst.
[0136] Comparative Example 6
[0137] This comparative example provides a catalyst, which is different from Example 1 only in that barium carbonate of the same particle size and mass is used instead of calcium carbonate.
[0138] Test Case
[0139] 1. Catalyst parameter test
[0140] The catalysts provided in each embodiment and comparative example were tested for physical and chemical properties, and the specific testing methods are as follows:
[0141] Specific surface area: tested using a specific surface area and pore size analyzer (Bjbuilder SSA−7000);
[0142] Total pore volume: tested using a specific surface area and pore size analyzer (Bjbuilder SSA−7000);
[0143] Mesopore volume: tested using a surface area and pore size analyzer (Bjbuilder SSA−7000);
[0144] Fe and N element content: tested using X-ray photoelectron spectroscopy (K-Alpha+ x);
[0145] Fe-N4 coordination: tested using X-ray photoelectron spectroscopy (K-Alpha+ x);
[0146] The specific test results are shown in the table below:
[0147] Table 1
[0148]
[0149] 2. Catalytic performance test
[0150] The catalyst provided in each embodiment and comparative example was loaded into a fixed bed reactor with a loading amount of 100 ml, and the ethylbenzene raw material and air were allowed to flow through the fixed bed reactor to undergo peroxidation to obtain ethylbenzene hydroperoxide. The reactor was connected in series with 6 reactors, and the air velocity of ethylbenzene was 0.05 h -1 ; The mass ratio of air to ethylbenzene was controlled to be 0.001; the reaction temperature was 145°C and the reaction pressure was 0.24MPaG. The products after the reaction were analyzed to obtain the ethylbenzene conversion rate and product selectivity data, as shown in the following table:
[0151] Table 2
[0152]
[0153] From the data in the above table, it can be seen that Example 2 has the best catalytic activity, with an ethylbenzene conversion rate of 65.5% and an ethylbenzene hydroperoxide selectivity of 96.6%. Its good catalytic activity is due to its large specific surface area and mesoporous volume. Secondly, it has a high content of iron and nitrogen elements, which makes its catalytic reaction have better catalytic activity. Examples 1 and 3 have lower loaded iron contents due to different addition ratios of their iron-containing precursors; and Examples 4 and 5 have lower nitrogen and iron atom deposition contents due to different deposition temperatures, resulting in reduced reaction conversion and selectivity.
[0154] Examples 6 and 7 were prepared using different precursors (in different proportions) and at different deposition temperatures. Under these preparation conditions, the specific surface area and iron / nitrogen content of the catalyst were lower than those of other examples, but still had considerable catalytic performance.
[0155] Comparative Example 1 was not doped with an iron-containing precursor, and the prepared C / N catalyst had almost no catalytic activity, and the ethylbenzene conversion rate was substantially the same as when no catalyst was added.
[0156] Comparative Example 2 used different carbon and nitrogen sources to prepare the catalyst, but such carbon and nitrogen sources were difficult to load on the calcium carbonate template during the vapor deposition process, resulting in a decrease in its specific surface area and a low metallic iron loading, resulting in a poor catalytic effect.
[0157] In Comparative Example 3, the prepared C / N template was used to rivet metallic iron. It was found that the prepared catalyst had a high iron content, but the iron existed in the form of nanoparticles and no Fe-N4 active sites were formed, resulting in poor catalytic effect.
[0158] Comparative Example 4 was not doped with nitrogen, and iron-carbon nanoparticles were formed at high temperature, but it did not have Fe-N4 active sites, resulting in poor catalytic effect.
[0159] Comparative Example 5 uses a different catalyst preparation method. This preparation method also prepares a catalyst with iron nanoparticles. The catalyst metal content is high, but no Fe-N4 active sites are formed, resulting in poor catalytic effect.
[0160] Comparative Example 6 uses a different template, barium carbonate. Experiments show that it is difficult for iron and nitrogen elements to deposit on the template, and the catalyst does not have a high specific surface area and pore volume, resulting in poor catalytic effect.
[0161] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. Application of a catalyst in ethylbenzene peroxidation reaction, It is characterized in that The catalyst has a hollow structure and is composed of a carbon material co-doped with iron and nitrogen. Among them, iron is in the form of Fe-N 4 Existence in coordinated form; The preparation method of the catalyst comprises the following steps: S1, mixing a carbon and nitrogen source with an iron source to obtain a mixed material, and depositing the mixed material on nano-calcium carbonate by chemical vapor deposition; the carbon and nitrogen source includes at least one of pyridine, pyrrole, and ethylenediamine; the iron source includes at least one of soluble iron sources; S2, removing the nano calcium carbonate by acid treatment to obtain the catalyst.
2. The use according to claim 1, It is characterized in that Based on the mass of the catalyst, the iron element accounts for 0.06%-0.10%, and the nitrogen element accounts for 10.0%-12.7%.
3. The use according to claim 1 or 2, It is characterized in that The specific surface area of the catalyst is 400 m 2 / g-470m 2 / g, and the total pore volume is 0.96cm 3 / g-1.69cm 3 / g, and the mesopore volume is 0.65cm 3 / g-1.05cm 3 / g.
4. A method for preparing a catalyst, It is characterized in that The steps include: S1, mixing a carbon and nitrogen source with an iron source to obtain a mixed material, and depositing the mixed material onto nano-calcium carbonate by chemical vapor deposition; Wherein, the carbon and nitrogen source includes at least one of pyridine, pyrrole, and ethylenediamine; the iron source includes at least one of soluble iron sources; The molar ratio of the carbon-nitrogen source to the iron source is 60-800:1; the average particle size of the nano-calcium carbonate is 100nm-150nm; The temperature of the chemical vapor deposition is 800°C-1000°C; the heating rate of the chemical vapor deposition is 10°C / min-30°C / min; the time of the chemical vapor deposition is 10min-60min; the gas velocity of the chemical vapor deposition is 80sccm-200sccm; S2, removing the nano calcium carbonate by acid treatment to obtain the catalyst.
5. The method for preparing the catalyst according to claim 4, It is characterized in that The iron source includes at least one of ferric chloride, ferric acetylacetonate, ferric acetate and ferric sulfate.
6. Use of a catalyst prepared by the preparation method according to any one of claims 4 to 5 in ethylbenzene peroxidation reaction.
7. The use according to claim 6, It is characterized in that The reaction temperature of the ethylbenzene peroxidation reaction is 125° C.-145° C., and the reaction pressure is 0.1 MPaG-0.3 MPaG.
Citation Information
Patent Citations
Iron-nitrogen double-doped hollow porous carbon sphere nano material and preparation method thereof
CN110170331A
Nano hollow Si@C@SiO2@C multi-layer structure composite microsphere, preparation method thereof and application
CN111416114A
Preparation of hydroperoxides
US4262143A
Method of preparing ethylbenzene hydroperoxide by liquid-phase peroxidation of ethylbenzene and preparation method of propylene oxide
WO2019119489A1