Porous hydroxyapatite nano-beam microsphere as well as preparation method and application thereof

By mixing a solution of phosphate and urea with a solution of calcium salt and chelating agent under low-temperature hydrothermal conditions to adjust the pH reaction, porous hydroxyapatite nanobeam microspheres similar to natural bone tissue were successfully obtained, solving the existing problem. The technology has solved the problems of complex processes and high-temperature sintering, and has achieved a good material for bone tissue repair and injection regeneration.

CN118851115APending Publication Date: 2024-10-29SHANGHAI JIAOTONG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410920413.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult to obtain porous hydroxyapatite materials similar in structure and size to natural bone tissue with existing technology, and common synthesis methods require a high-temperature sintering process, which is cumbersome and difficult to avoid high-temperature heat treatment.

Method used

By mixing the first solution including phosphate and urea with the second solution including calcium salt and chelating agent, adjusting the pH and reacting, porous hydroxyapatite nanobeam microspheres are obtained. Low-temperature hydrothermal conditions are used to control the reaction and avoid high temperatures. sintering.

Benefits of technology

Porous hydroxyapatite nanobeam microspheres with a structure similar to natural bone tissue can be obtained quickly and simply. They have good osteoconductivity, bioactivity and biocompatibility, and are suitable for bone tissue repair and injection regeneration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004936522040000011
    Figure HDA0004936522040000011
  • Figure HDA0004936522040000012
    Figure HDA0004936522040000012
  • Figure HDA0004936522040000021
    Figure HDA0004936522040000021
Patent Text Reader

Abstract

The invention relates to the technical field of new materials, in particular to a porous hydroxyapatite nano-beam microsphere as well as a preparation method and application thereof. The preparation method of the porous hydroxyapatite nano-beam microspheres comprises the following steps: mixing a first solution containing phosphate and urea with a second solution containing calcium salt and a chelating agent, adjusting the pH value, carrying out a reaction, and washing and drying a precipitate obtained by the reaction to obtain the porous hydroxyapatite nano-beam microspheres. When the structure and the size of the obtained porous hydroxyapatite nano-beam microspheres are similar to those of hydroxyapatite in natural bone tissue, the porous hydroxyapatite nano-beam microspheres have the advantages of being good in osteoconductivity, biological activity and biocompatibility, capable of promoting collagen regeneration and the like, and are good materials for bone tissue repair and injection regeneration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new materials, and in particular to porous hydroxyapatite nanobeam microspheres and a preparation method and application thereof. Background Art

[0002] The inorganic components of human bone tissue are mainly hydroxyapatite. When the structure and size of artificially synthesized hydroxyapatite are similar to those of hydroxyapatite in natural bone tissue, it has the advantages of good osteoconductivity, bioactivity, biocompatibility, and promotion of collagen regeneration, and is a good material for bone tissue repair and injection regeneration. However, most of the common hydroxyapatite synthesis methods currently rely on high-temperature sintering to obtain hydroxyapatite with a good crystal phase, and the sintering recrystallization process often makes hydroxyapatite present a dense block morphology, making it difficult to obtain hydroxyapatite similar to the structure of natural bone tissue. Therefore, it is still particularly important to obtain hydroxyapatite materials with porous morphology and a certain similarity to the structure and size of natural bone tissue.

[0003] At present, there are also some studies on the preparation of porous hydroxyapatite particles, but most of these processes are relatively cumbersome. For example, microemulsion method and spray drying technology, both of which require the synthesis of hydroxyapatite precipitation, and then a secondary molding process to obtain porous or solid microspheres with a certain morphology, and finally, high-temperature sintering is required to remove the additives. It is difficult to avoid the high-temperature heat treatment process in the conventional synthesis process. Therefore, the development of a new preparation method for hydroxyapatite microspheres is an urgent problem to be solved in current research. Summary of the invention

[0004] In view of the problems existing in the prior art, the first aspect of the present invention provides a method for preparing porous hydroxyapatite nanobeam microspheres, comprising the following steps: mixing a first solution containing phosphate and urea with a second solution containing a calcium salt and a chelating agent, reacting after adjusting the pH, washing and drying the precipitate obtained by the reaction, and obtaining the porous hydroxyapatite nanobeam microspheres.

[0005] Preferably, A1) the phosphate is selected from one or more of (NH4)2HPO4, (NH4)H2PO4, Na2HPO4, NaH2PO4, K2HPO4, KH2PO4;

[0006] Preferably, the mass ratio of the phosphate to urea in A2) is 1:(0.1-12), for example, it can be 1:(0.1-2), 1:(2-4), 1:(4-6), 1:(6-8), 1:(8-10) or 1:(10-12), etc.

[0007] Preferably, the calcium salt in A3) is selected from one or more of Ca(NO3)2.4H2O, CaCl2.2H2O, calcium acetate and calcium formate;

[0008] Preferably, the chelating agent A4) is selected from one or more of disodium ethylenediaminetetraacetate (Na2EDTA), tartaric acid, sodium citrate, and citric acid;

[0009] Preferably, the mass ratio of the calcium salt to the chelating agent in A5) is 1:(0.01-10), for example, it can be 1:(0.01-0.1), 1:(0.1-2), 1:(2-4), 1:(4-6), 1:(6-8), 1:(8-10) or 1:(10-12), etc.;

[0010] Preferably, A6) the solvent of the first solution is water;

[0011] Preferably, A7) the solvent of the second solution is water.

[0012] Preferably, when the first solution and the second solution are mixed, the mass ratio of Ca to P is (1-10):1, for example, (1-2:1), (2-3:1), (3-4:1), (4-5:1), (5-6:1), (6-7:1), (7-8:1),

[0013] 1), (8-9:1) or (9-10:1), etc.

[0014] Preferably, the pH is adjusted to between 1 and 3.5 or between 10 and 14. Under acidic and alkaline conditions, the equilibrium state can be changed by degradation of some substances in the reaction system, thereby precipitating porous hydroxyapatite nanobeam microspheres. For example, the pH can be 1-2, 2-3, 3-3.5, 10-11, 11-12, 12-13, 13-14.

[0015] Preferably, the pH adjusting agent is selected from inorganic acids or bases.

[0016] Preferably, B1) the inorganic acid is selected from one or more of nitric acid, hydrochloric acid or sulfuric acid;

[0017] Preferably, the base in B2) is selected from aqueous ammonia or caustic soda solution.

[0018] Preferably, the reaction temperature in C1) is 80-250°C, for example, 80-100°C, 100-120°C, 120-140°C, 140-160°C, 160-180°C, 180-200°C, 200-220°C, 220-240°C, 240-250°C, etc.

[0019] Preferably, the reaction time of C2) is 3 to 24 hours; in the present invention, the reaction time and the reaction temperature cooperate with each other. Under low temperature conditions, a longer reaction time is required, and under high temperature conditions, the reaction time is relatively shortened. Under different temperature / time reaction conditions, the particle size of the obtained spheres is also different. Under the reaction temperature and reaction time specified in the present invention, the obtained porous hydroxyapatite nanobeam microspheres are similar in structure and size to the hydroxyapatite in natural bone tissue, and have good bone conductivity, biological activity, biocompatibility, and the advantages of promoting collagen regeneration, and are good materials for bone tissue repair and injection regeneration.

[0020] Preferably, the equipment for the reaction in C3) is a closed pressure-resistant container.

[0021] Preferably, the drying temperature is ≤80°C.

[0022] In the present invention, the degradation of urea in the reaction system is controlled by temperature and time, and the gas generated by the degradation is used to change the equilibrium state of the sealed reaction system, thereby generating hydroxyapatite porous microsphere deposition.

[0023] The second aspect of the present invention provides porous hydroxyapatite nanobeam microspheres, which are prepared by the above-mentioned preparation method of porous hydroxyapatite nanobeam microspheres. The hydroxyapatite composite nanobeam microspheres prepared by the method of the present invention have a uniform size distribution range of 1 to 60 μm and a central particle size of 20-60 μm.

[0024] The third aspect of the present invention provides the use of the porous hydroxyapatite nanobeam microspheres in human bones.

[0025] About 30% of natural bones are collagen, and about 70% are hydroxyapatite (HA). Nano-sheet HA and collagen are assembled into bone lamellae, and the 3-7μm thick bone lamellae are arranged in phase to form a Haversian system. A single Haversian system is a cylinder with a size between 10-100μm, a hollow tube (Havers tube) running through the center, and blood vessels inside to provide material exchange channels for the surrounding bone tissue. The Haversian system is the basic unit of natural bones, and its micron-scale size and high connectivity are the key to maintaining bone health. The porous hydroxyapatite nanobeam microspheres obtained in the present invention are similar in size to the Haversian system, and both are assembled from HA nanosheets in microstructure, and the inorganic component (HA) is consistent. In addition, gaps can be spontaneously formed between the tightly packed HA microspheres, combined with the porous characteristics of the HA microspheres themselves, which can imitate the interconnected structure of the Haversian system to a certain extent. Therefore, the porous hydroxyapatite nanobeam microspheres in the present invention can simulate natural bones in terms of physical structure and chemical composition.

[0026] The present invention has the following beneficial effects:

[0027] 1) Compared with the existing preparation process, the process of the present invention is simple, and hydroxyapatite nanobeam microspheres can be obtained by a quick precipitation.

[0028] 2) The porous hydroxyapatite nanospheres obtained by the present invention have similar structures and sizes to the hydroxyapatite in natural bone tissue, and have the advantages of good osteoconductivity, bioactivity, biocompatibility and promoting collagen regeneration, and are good materials for bone tissue repair and injection regeneration. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a low magnification SEM image of the porous hydroxyapatite nanobeam microspheres in Example 1 of the present invention, with the magnification being 150 times.

[0030] Figure 2 : is the size distribution of the porous hydroxyapatite nanobeam microspheres in Example 1 of the present invention.

[0031] Figure 3 This is a high-magnification SEM image of the porous hydroxyapatite nanobeam microspheres in Example 1 of the present invention, with the magnification being 10,000 times.

[0032] Figure 4 This is a high-magnification SEM image of the porous hydroxyapatite nanobeam microspheres in Example 2 of the present invention, with the magnification being 10,000 times.

[0033] Figure 5 This is a high-magnification SEM image of the porous hydroxyapatite nanobeam microspheres in Example 3 of the present invention, with the magnification being 1000 times.

[0034] Figure 6 This is a high-magnification SEM image of the porous hydroxyapatite nanobeam microspheres in Example 4 of the present invention, with the magnification being about 1000 times.

[0035] Figure 7 This is a high-magnification SEM image of the porous hydroxyapatite nanobeam microspheres in Example 5 of the present invention, with the magnification being 1000 times. DETAILED DESCRIPTION

[0036] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0037] See also Figure 1 to Figure 2. It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings in this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any modification of the structure, change in the proportional relationship, or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the implementation of the present invention without substantially changing the technical content.

[0038] It should be noted that Urea in the following examples refers to urea.

[0039] Example 1

[0040] Step 1 Solution preparation:

[0041] First solution: 0.9508 g (NH4)2HPO4 and 0.2883 g Urea were dissolved in 30 mL deionized water to obtain a first solution;

[0042] Second solution: 2.8338 g of Ca(NO3)2.4H2O was dissolved in 30 mL of deionized water and then 4.5 g of Na2EDTA.2H2O was added to obtain a second solution;

[0043] Step 2 Solution mixing:

[0044] Add the first solution in step 1 dropwise into the second solution while stirring continuously;

[0045] Step 3 pH adjustment:

[0046] Adjust the pH of the mixture in step 2 to 14 with 10M NaOH, 1M NaOH and 1M HNO3;

[0047] Step 4 Solution transfer and hydrothermal:

[0048] Transfer the solution in step 3 to a hydrothermal reactor and place it in an oven heated to 80°C for 24 hours.

[0049] Step 5 Material collection and washing:

[0050] After the reaction was completed, the reactor was cooled to room temperature, samples were collected, washed with a large amount of deionized water, and freeze-dried.

[0051] The morphology of the obtained HA microspheres was observed using SEM, and the size distribution of the obtained HA microspheres was obtained using a laser particle size analyzer.

[0052] Figure 1 This is a low magnification SEM image of the porous hydroxyapatite nanobeam microspheres with high specific surface area obtained in Example 1. It can be seen that the porous hydroxyapatite nanobeam microspheres are spherical and have uniform sizes of 1 to 60 μm. Figure 2 This is the size distribution of the porous hydroxyapatite nanobeam microspheres with high specific surface area obtained in Example 1. It can be seen that the average diameter of the microspheres is 32.75±14.60 μm, and the size presents a single distribution. Figure 3 This is a high magnification SEM image of the porous hydroxyapatite nanobeam microspheres with high specific surface area obtained in Example 1. It can be seen that the microspheres are assembled from nanosheets of the porous hydroxyapatite nanobeam microspheres, and there are pores between the nanosheets, which proves that the obtained porous hydroxyapatite nanobeam microspheres have a porous structure.

[0053] About 30% of natural bones are collagen and about 70% are HA. Nano-sheet HA and collagen are assembled into bone lamellae, and 3-7 μm thick bone lamellae are arranged in phase to form a Haversian system. A single Haversian system is a cylinder with a size between 10-100 μm, a hollow tube (Havers tube) running through the center, and blood vessels passing through it to provide material exchange channels for the surrounding bone tissue. The Haversian system is the basic unit of natural bones, and its micron-scale size and high connectivity are the key to maintaining bone health. The porous hydroxyapatite nanobeam microspheres obtained in Example 1 are similar in size to the Haversian system, and both are assembled from HA nanosheets in microstructure, and the inorganic component (HA) is consistent. In addition, gaps can be spontaneously formed between the tightly packed HA microspheres, combined with the porous characteristics of the HA microspheres themselves, which can imitate the interconnected structure of the Haversian system to a certain extent. Therefore, the porous hydroxyapatite nanobeam microspheres in this embodiment can simulate natural bones in terms of physical structure and chemical composition.

[0054] Example 2

[0055] Step 1 Solution preparation:

[0056] First solution: 0.9508 g (NH4)2HPO4 and 0.2883 g Urea were dissolved in 30 mL deionized water to obtain a second solution;

[0057] Second solution: Dissolve 2.8338 g of Ca(NO3)2.4H2O in 30 mL of deionized water and add 4.5 g of Na2EDTA.2H2O to obtain a second solution;

[0058] Step 2 Solution mixing:

[0059] Add the first solution in step 1 dropwise into the second solution while stirring continuously;

[0060] Step 3 pH adjustment:

[0061] Adjust the pH of the mixture in step 2 to 10 with 10M NaOH, 1M NaOH and 1M HNO3;

[0062] Step 4 Solution transfer and hydrothermal:

[0063] Transfer the solution in step 3 to a hydrothermal reactor and place it in an oven heated to 250°C for 3 hours.

[0064] Step 5 Material collection and washing:

[0065] After the reaction was completed, the reactor was cooled to room temperature, samples were collected, washed with a large amount of deionized water, and freeze-dried.

[0066] The morphology of the obtained HA microspheres was observed using SEM.

[0067] Figure 4 This is a high magnification SEM image of the high specific surface area HA microspheres obtained in Example 2. It can be seen that the HA microspheres are spherical and assembled from flaky HA particles with a diameter of about 15 μm. Compared with Example 1, due to the higher hydrothermal reaction temperature, the HA growth rate is accelerated and the HA particle size is larger. Some HA particles grow excessively, destroying the microsphere morphology and blocking the pores in the microspheres.

[0068] Example 3

[0069] Step 1 Solution preparation:

[0070] Solution a: Dissolve 2.8338 g of Ca(NO3)2.4H2O in 30 mL of deionized water;

[0071] Solution b: Dissolve 0.9508 g (NH4)2HPO4 in 30 mL deionized water;

[0072] Step 2 Solution mixing:

[0073] Add solution b in step 1 dropwise into solution a while stirring continuously;

[0074] Step 3 pH adjustment:

[0075] Adjust the pH of the mixture in step 2 to 1 with 1M HNO3 and 5M HNO3, then add the corresponding amount of Na2EDTA.2H2O and Urea and continue to adjust the pH to 3;

[0076] Step 4 Solution transfer and hydrothermal:

[0077] Transfer the solution in step 3 to a hydrothermal reactor and place it in an oven heated to 80°C for 24 hours.

[0078] Step 5 Material collection and washing:

[0079] After the reaction was completed, the reactor was cooled to room temperature, samples were collected, washed with deionized water, centrifuged three times, and freeze-dried.

[0080] The morphology of the obtained HA microspheres was observed using SEM.

[0081] Figure 5 This is a high magnification SEM image of the high specific surface area HA microspheres obtained in Example 3. It can be seen that the HA microspheres are small in size, about 2-5 μm in diameter, and nearly spherical in shape, and are assembled from nano HA particles. Compared with Example 1, due to the lower hydrothermal reaction temperature, the HA growth rate is slower, and there are more nucleation sites in the solution system, resulting in smaller HA particle size. The nano HA particles are not grown enough and lack mutual connection, so the microsphere morphology is poorer in sphericity than in Example 1.

[0082] Example 4

[0083] Step 1 Solution preparation:

[0084] Solution a: Dissolve 2.8338 g of Ca(NO3)2.4H2O in 30 mL of deionized water;

[0085] Solution b: Dissolve 0.9508 g (NH4)2HPO4 in 30 mL deionized water;

[0086] Step 2 Solution mixing:

[0087] Add solution b in step 1 dropwise into solution a while stirring continuously;

[0088] Step 3 pH adjustment:

[0089] Adjust the pH of the mixture in step 2 to 1 with 1M HNO3 and 5M HNO3, then add the corresponding amount of Na2EDTA.2H2O and Urea and continue to adjust the pH to 3;

[0090] Step 4 Solution transfer and hydrothermal:

[0091] Transfer the solution in step 3 to a hydrothermal reactor and place it in an oven heated to 250°C for 3 hours.

[0092] Step 5 Material collection and washing:

[0093] After the reaction was completed, the reactor was cooled to room temperature, samples were collected, washed with deionized water, centrifuged three times, and freeze-dried.

[0094] The morphology of the obtained HA microspheres was observed using SEM.

[0095] Figure 6 This is a high magnification SEM image of the high specific surface area HA microspheres obtained in Example 4. It can be seen that the HA microspheres are spherical, with a diameter between 10-50 μm, and are assembled from nano HA particles. Compared with Example 1, at a lower pH and higher hydrothermal temperature, the HA particles maintain a more suitable growth rate, and finally assemble into microspheres, and the pore structure between the lamellar HA particles is still maintained.

[0096] Example 5

[0097] Step 1 Solution preparation:

[0098] Solution a: Dissolve 2.8338 g of Ca(NO3)2.4H2O in 30 mL of deionized water;

[0099] Solution b: Dissolve 0.9508 g (NH4)2HPO4 in 30 mL deionized water;

[0100] Step 2 Solution mixing:

[0101] Add solution b in step 1 dropwise into solution a while stirring continuously;

[0102] Step 3 pH adjustment:

[0103] Adjust the pH of the mixture in step 2 to 7 with 1M HNO3 and 5M HNO3, then add the corresponding amount of Na2EDTA.2H2O and Urea and continue to adjust the pH to 3;

[0104] Step 4 Solution transfer and hydrothermal:

[0105] Transfer the solution in step 3 to a hydrothermal reactor and place it in an oven heated to 80°C for 24 hours.

[0106] Step 5 Material collection and washing:

[0107] After the reaction was completed, the reactor was cooled to room temperature, samples were collected, washed with deionized water, centrifuged three times, and freeze-dried.

[0108] The morphology of the obtained HA microspheres was observed using SEM.

[0109] Figure 7 This is a high magnification SEM image of the high specific surface area HA microspheres obtained in Example 5. It can be seen that the HA microspheres are spherical, with a diameter of 5-10 μm, and are assembled from flaky nano HA particles. Compared with Example 1, at a higher pH and lower hydrothermal temperature, the HA particles maintained a more suitable growth rate, and finally assembled into microspheres, and the pore structure between the flaky HA particles was still maintained.

[0110] The above examples achieve controllable preparation of porous HA nanobeam microspheres by using different hydrothermal reaction temperatures, pH and Na2EDTA·2H2O / Urea addition sequences. The HA microspheres prepared in this way are similar to HA in natural bone tissue and can simulate natural bone tissue. In theory, they have good osteoconductivity, bioactivity, biocompatibility and the advantages of promoting collagen regeneration, and are expected to be used as a good material for bone tissue repair and injection regeneration.

[0111] The above description is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and equivalent changes made by using the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing porous hydroxyapatite nanobeam microspheres, It is characterized in that include: The first solution containing phosphate and urea is mixed with the second solution containing calcium salt and chelating agent, and reacted after adjusting the pH, and the precipitate obtained by the reaction is washed and dried to obtain the porous hydroxyapatite nanobeam microspheres.

2. The method for preparing porous hydroxyapatite nanospheres according to claim 1, It is characterized in that Include at least one of the following technical features: A1) the phosphate is selected from (NH 4 ) 2 HPO 4 NH 4 )H 2 PO 4 、Na 2 HPO 4 、NaH 2 PO 4 , K 2 HPO 4 , KH 2 PO 4 One or more of the following; A2) the mass ratio of the phosphate to the urea is 1:(0.1-12); A3) The calcium salt is selected from Ca(NO 3 ) 2 .4H 2 O, CaCl 2 ·2H 2 O, one or more of calcium acetate and calcium formate; A4) The chelating agent is selected from disodium ethylenediaminetetraacetate (Na 2 EDTA), tartaric acid, sodium citrate, citric acid, one or more thereof; A5) the mass ratio of the calcium salt to the chelating agent is 1:(0.01-10); A6) the solvent of the first solution is water; A7) The solvent of the second solution is water.

3. The method for preparing porous hydroxyapatite nanospheres according to claim 1, It is characterized in that When the first solution and the second solution are mixed, the mass ratio of Ca to P is (1-10):

1.

4. The method for preparing porous hydroxyapatite nanospheres according to claim 1, It is characterized in that The pH is adjusted to one selected from 1 to 3.5 or 10 to 14.

5. The method for preparing porous hydroxyapatite nanospheres according to claim 4, It is characterized in that The pH adjusting agent is selected from inorganic acids or bases.

6. The method for preparing porous hydroxyapatite nanobeam microspheres according to claim 5, It is characterized in that Includes one of the following technical features: B1) the inorganic acid is selected from one or more of nitric acid, hydrochloric acid or sulfuric acid; B2) The alkali is selected from aqueous ammonia or caustic soda solution.

7. The method for preparing porous hydroxyapatite nanobeam microspheres according to claim 1, It is characterized in that Includes one of the following technical features: C1) the reaction temperature is 80 to 250°C; C2) the reaction time is 3 to 24 hours; C3) The equipment for the reaction is a closed pressure-resistant container.

8. The method for preparing porous hydroxyapatite nanobeam microspheres according to claim 1, It is characterized in that The drying temperature is ≤80°C.

9. A porous hydroxyapatite nanobeam microsphere, It is characterized in that The porous hydroxyapatite nanobeam microspheres are prepared by the preparation method of any one of claims 1 to 8.

10. Use of the porous hydroxyapatite nanobeam microspheres according to claim 9 in human bones.

Citation Information

Patent Citations

  • Porous hydroxyapatite microsphere material and preparation method thereof

    CN115108542A

  • Hydroxyapatite microspheres as well as preparation method and application thereof

    CN118206089A

  • Preparation method of fluorine-containing hydroxyapatite nanorod assembled microspheres

    CN118221097A