Synthetic quartz and preparation method thereof
Through multi-step processing of the silicon source, synthetic quartz with excellent transmittance in the ultraviolet and vacuum ultraviolet bands is prepared, which solves the problem of insufficient transmittance of existing quartz and realizes wide application in high-tech fields.
Patent Information
- Application Number
- CN202310416061.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-29
AI Technical Summary
Existing synthetic quartz has low transmittance in the external and vacuum ultraviolet bands, which limits its application in high-tech industries.
By subjecting the silicon source to deposition, dehydroxylation, inert gas replacement, oxidation, sintering, annealing and hydrogen-based gas treatment, synthetic quartz with excellent transmittance is prepared. The specific steps include step-by-step processing in a vacuum environment. Simultaneous heating and sintering Perform hydrogen gas treatment to control the content of SiO2, hydroxyl, chlorine, fluorine, hydrogen, deuterium, silicon-hydrogen bonds, oxygen vacancies, peroxide defects, alkali metal elements and transition metal elements to ensure that the synthetic quartz performs well in the ultraviolet band and High transmittance in the vacuum ultraviolet band.
It achieves excellent transmittance of synthetic quartz in the ultraviolet band and vacuum ultraviolet band, and reduces stress birefringence and optical non-uniformity. It is suitable for ultraviolet optical and vacuum ultraviolet optical components, and the preparation process is simple and suitable for a wide range of applications.
Smart Images

Figure BDA0004188398990000141 
Figure BDA0004188398990000144 
Figure BDA0004188398990000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material preparation, and in particular to synthetic quartz and a preparation method thereof. Background Art
[0002] Synthetic quartz is an amorphous material with a single component of silicon dioxide. It has excellent physical and chemical properties and is an ideal optical material. Synthetic quartz is widely used in high-tech industries such as microelectronics, precision optics, space technology and laser technology. However, the existing synthetic quartz has low transmittance in the outer band and vacuum ultraviolet band, which greatly limits the further application of synthetic quartz. Therefore, it is urgent to provide a synthetic quartz with excellent transmittance in the outer band and vacuum ultraviolet band. Summary of the invention
[0003] The invention provides a synthetic quartz having excellent transmittance in both the ultraviolet band (10-380nm) and the vacuum ultraviolet band (10-195nm).
[0004] The invention provides a method for preparing synthetic quartz. The method can prepare the synthetic quartz mentioned above, and the preparation process is simple and suitable for wide popularization and application.
[0005] The present invention provides a synthetic quartz, wherein the stress birefringence of the synthetic quartz to light with a wavelength of 633 nm is ≤1.6 nm / cm, and the optical inhomogeneity to light with a wavelength of 633 nm is ≤2.1×10 -6 ;
[0006] The synthetic quartz having a thickness of 10 mm has an initial internal transmittance of ≥99.6% for light having a wavelength of 193 nm, and an initial internal transmittance of ≥88.3% for light having a wavelength of 157 nm.
[0007] The synthetic quartz as described above, wherein the synthetic quartz with a thickness of 10 mm, has a wavelength of 193 nm and an energy of 10 mJ / cm 2 , the pulse is 2×10 6 After light irradiation, the internal transmittance decreases by ≤0.6%.
[0008] The synthetic quartz as described above, wherein the synthetic quartz
[0009] The mass percentage of SiO2 is greater than 99.999%;
[0010] The mass percentage of hydroxyl is 0.1-50ppm;
[0011] The mass percentage of chlorine element is less than 10ppm;
[0012] The content of fluorine is 0.1-2 mol / cm 3 ;
[0013] The sum of the contents of hydrogen and deuterium is 1×10 15 -2×10 18 molecules / cm 3 ;
[0014] The content of silicon-hydrogen bonds is less than 2×10 17 Pieces / cm 3 ;
[0015] The content of oxygen vacancies is less than 1×10 16 Pieces / cm 3 ;
[0016] The content of peroxygen defects is less than 1×10 16 Pieces / cm 3 ;
[0017] The mass percentage of alkali metal elements is less than 20ppb;
[0018] The mass percentage of alkaline earth metal elements is less than 10ppb;
[0019] The mass percentage of transition metal elements is less than 20ppb.
[0020] The synthetic quartz as described above, wherein the synthetic quartz
[0021] The mass percentage of SiO2 is greater than 99.9997%;
[0022] The mass percentage of hydroxyl is 10-30ppm;
[0023] The mass percentage of chlorine element is less than 2ppm;
[0024] The content of fluorine is 0.6-1 mol / cm 3 ;
[0025] The sum of the contents of hydrogen and deuterium is 2×10 16 -2×10 17 molecules / cm 3 ;
[0026] The content of silicon-hydrogen bonds is less than 1×10 16 molecules / cm 3 ;
[0027] The content of oxygen vacancies is less than 1×10 15 Pieces / cm 3 ;
[0028] The content of peroxygen defects is less than 1×10 15 Pieces / cm 3;
[0029] The mass percentage of alkali metal elements is less than 5ppb;
[0030] The mass percentage of alkaline earth metal elements is less than 2ppb;
[0031] The mass percentage of transition metal elements is less than 5ppb.
[0032] The present invention provides a method for preparing the synthetic quartz as described above, which comprises the following steps:
[0033] Performing deposition treatment on a silicon source to obtain a silicon dioxide preform;
[0034] The synthetic quartz is obtained by sequentially subjecting the silicon dioxide preform to dehydroxylation treatment, inert gas replacement treatment, oxidation treatment, sintering treatment, annealing treatment and hydrogen-based gas treatment.
[0035] The preparation method as described above, wherein, in the deposition process, the temperature is 1000-1200° C. and the pressure is -80 to -20 Pa; and / or,
[0036] In the deposition process, the combustion gas includes hydrogen and oxygen, and the equivalent volume ratio of hydrogen to oxygen in the combustion gas is (2.1-2.8):1; and / or,
[0037] In the dehydroxylation treatment, the temperature is 1100-1300° C. and the time is 4-40 hours.
[0038] The preparation method as described above, wherein, in the inert gas replacement treatment, the pressure is 100-10000 Pa, the time is 1-10 hours, and the temperature is 1100-1300° C.; and / or,
[0039] In the oxidation treatment, the temperature is 1000-1400° C., the oxygen partial pressure is 100-10000 Pa, the mass percentage of water in the oxygen is less than 1 ppm, and the time is 1-5 hours.
[0040] The preparation method as described above, wherein the sintering process sequentially comprises:
[0041] Under a vacuum degree of ≤10 Pa, heating the oxidized silicon dioxide preform from 0° C. to 1000° C. at a rate of 100-500° C. / h to obtain a first sintered preform;
[0042] Under a vacuum degree of ≤5 Pa, heating the first sintered preform from 1000° C. to 1300° C. at a rate of 2-5° C. / h to obtain a second sintered preform;
[0043] Under a vacuum degree of ≤2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 6-10° C. / h to obtain a third sintered preform;
[0044] The third sintered preform is sintered at a vacuum degree of ≤1 Pa and a temperature of 1500° C. for 1-2 hours to obtain a synthetic quartz blank.
[0045] In the preparation method as described above, the annealing treatment comprises: heat-insulating the synthetic quartz body at 1050°C-1300°C, cooling it to 800-900°C at a cooling rate of less than or equal to 2°C / h, and naturally cooling it to room temperature.
[0046] As described above, in the preparation method, in the hydrogen-based gas treatment, the volume percentage of the hydrogen-based gas is 5-100%, the temperature is 300-500° C., the pressure is 0.1-1 MPa, and the time is 5-100 h.
[0047] The invention provides a synthetic quartz having lower stress birefringence and optical inhomogeneity and excellent transmittance to light above 157nm in the ultraviolet band and the vacuum ultraviolet band.
[0048] The invention provides a method for preparing synthetic quartz. The method can prepare synthetic quartz with excellent transmittance in an ultraviolet band of 157 nm and above and a vacuum ultraviolet band, and the method has a simple preparation process and is suitable for wide promotion and application. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0050] The first aspect of the present invention provides a synthetic quartz, wherein the stress birefringence of the synthetic quartz to light with a wavelength of 633 nm is ≤1.6 nm / cm, and the optical inhomogeneity to light with a wavelength of 633 nm is ≤2.1×10 -6 ;
[0051] The initial internal transmittance of synthetic quartz with a thickness of 10 mm for light with a wavelength of 193 nm is ≥ 99.6%, and the initial internal transmittance for light with a wavelength of 157 nm is ≥ 88.3%.
[0052] In the present invention, synthetic quartz will undergo stress birefringence due to photoelastic action under mechanical stress, and stress birefringence can show the anisotropy of synthetic quartz and reflect the internal stress distribution of synthetic quartz. Optical non-uniformity refers to the degree of unevenness of the refractive index change of each part in synthetic quartz. When light enters synthetic quartz, reflection, absorption and transmission will occur. The internal transmittance of light is obtained by correcting the external transmittance of light for reflection loss, which can accurately reflect the optical transmittance of synthetic quartz.
[0053] The synthetic quartz of the present invention has lower stress birefringence and optical inhomogeneity and excellent initial internal transmittance, and therefore can be widely used in ultraviolet optical components and vacuum ultraviolet optical components.
[0054] In some embodiments of the present invention, synthetic quartz with a thickness of 10 mm, a wavelength of 193 nm, and an energy of 10 mJ / cm 2 , the pulse is 2×10 6 After light irradiation, the internal transmittance decreases by ≤0.6%.
[0055] The internal transmittance decrease value refers to the difference between the initial internal transmittance of synthetic quartz to light with a wavelength of 193nm before irradiation and the irradiated internal transmittance of synthetic quartz to light with a wavelength of 193nm after irradiation. During use, the synthetic quartz of the present invention has a lower internal transmittance decrease value and less internal transmittance attenuation.
[0056] In some embodiments of the present invention, in the synthetic quartz,
[0057] The mass percentage of SiO2 is greater than 99.999%;
[0058] The mass percentage of hydroxyl is 0.1-50ppm;
[0059] The mass percentage of chlorine element is less than 10ppm;
[0060] The content of fluorine is 0.1-2 mol / cm 3 ;
[0061] The sum of the contents of hydrogen and deuterium is 1×10 15 -2×10 18 molecules / cm 3 ;
[0062] The content of silicon-hydrogen bonds is less than 2×10 17 Pieces / cm 3 ;
[0063] The content of oxygen vacancies is less than 1×10 16 Pieces / cm 3 ;
[0064] The content of peroxygen defects is less than 1×10 16 Pieces / cm 3 ;
[0065] The mass percentage of alkali metal elements is less than 20ppb;
[0066] The mass percentage of alkaline earth metal elements is less than 10ppb;
[0067] The mass percentage of transition metal elements is less than 20ppb.
[0068] In the present invention, the mass percentage of SiO2 in synthetic quartz refers to the ratio of the mass of SiO2 in synthetic quartz to the total mass of synthetic quartz, which can be obtained by the loss on ignition method (GB / T3284-2015); the mass percentage of hydroxyl in synthetic quartz refers to the ratio of the mass of hydroxyl in synthetic quartz to the total mass of synthetic quartz, which can be obtained by spectrophotometry; the mass percentage of chlorine in synthetic quartz refers to the ratio of the mass of chlorine in synthetic quartz to the total mass of synthetic quartz, which can be obtained by X-ray fluorescence spectroscopy; the content of fluorine in synthetic quartz refers to the molar content of fluorine in unit volume of synthetic quartz, which can be obtained by X-ray fluorescence spectroscopy. The synthetic quartz of the present invention has gaps between SiO2 molecules, and the gaps are filled with hydrogen and / or tritium. The sum of the contents of hydrogen and deuterium in the synthetic quartz refers to the total number of hydrogen molecules and tritium molecules in a unit volume of the synthetic quartz, which can be obtained by Raman spectroscopy. The content of silicon-hydrogen bonds in the synthetic quartz refers to the number of silicon-hydrogen bonds in a unit volume of the synthetic quartz, the content of oxygen vacancies in the synthetic quartz refers to the number of ≡Si-Si≡ bonds in a unit volume of the synthetic quartz, and the content of peroxygen defects in the synthetic quartz refers to the number of ≡Si-O-O-Si≡ bonds in a unit volume of the synthetic quartz. The content of silicon-hydrogen bonds, the content of oxygen vacancies in the synthetic quartz, and the content of peroxygen defects can all be measured by "Reaction The alkali metal elements in synthetic quartz include Li, Na and K, and the mass percentage of the alkali metal elements refers to the ratio of the total mass of the alkali metal elements in the synthetic quartz to the total mass of all elements in the synthetic quartz, and the mass percentage of the alkali metal elements can be obtained by inductively coupled plasma mass spectrometry; the alkaline earth metal elements in synthetic quartz include Mg and Ca, and the mass percentage of the alkaline earth metal elements refers to the ratio of the total mass of the alkaline earth metal elements in the synthetic quartz to the total mass of all elements in the synthetic quartz, and the mass percentage of the alkaline earth metal elements can be obtained by inductively coupled plasma mass spectrometry; the transition metal elements in synthetic quartz include Ti, Cr, Fe, Ni, Cu, Zr and Mo, and the mass percentage of the transition metal elements refers to the ratio of the total mass of the transition metal elements in the synthetic quartz to the total mass of all elements in the synthetic quartz, and the content of the transition metal elements can be obtained by inductively coupled plasma mass spectrometry.
[0069] Since the synthetic quartz of the present invention contains specific contents of SiO2, hydroxyl, chlorine, fluorine, hydrogen, deuterium, silicon-hydrogen bonds, oxygen vacancies, peroxygen defects, alkali metal elements, alkaline earth metal elements and transition metal elements, the synthetic quartz has excellent transmittance in the ultraviolet band and the vacuum ultraviolet band, and the synthetic quartz also has lower optical non-uniformity and lower stress birefringence in the ultraviolet band and the vacuum ultraviolet band.
[0070] It is worth mentioning that the specific content of fluorine, hydrogen, deuterium, silicon-hydrogen bonds, oxygen vacancies, peroxide defects, alkali metals, alkaline earth metals and transition metals in synthetic quartz can also make synthetic quartz have a wavelength of 193nm and an energy of 10mJ / cm 2 , the pulse is 2×10 6 After being irradiated by light, the internal transmittance decreases by no more than 0.2%. The synthetic quartz of the invention can be widely used in ultraviolet optical components and vacuum ultraviolet optical components.
[0071] In some embodiments of the present invention, when the synthetic quartz,
[0072] The mass percentage of SiO2 is greater than 99.9997%;
[0073] The mass percentage of hydroxyl is 10-30ppm;
[0074] The mass percentage of chlorine element is less than 2ppm;
[0075] The content of fluorine is 0.6-1 mol / cm 3 ;
[0076] The sum of the contents of hydrogen and deuterium is 2×10 16 -2×10 17 molecules / cm 3 ;
[0077] The content of silicon-hydrogen bonds is less than 1×10 16 Pieces / cm 3 ;
[0078] The content of oxygen vacancies is less than 1×10 15 Pieces / cm 3 ;
[0079] The content of peroxygen defects is less than 1×10 15 Pieces / cm 3 ;
[0080] The mass percentage of alkali metal elements is less than 5ppb;
[0081] The mass percentage of alkaline earth metal elements is less than 2ppb;
[0082] When the mass percentage content of the transition metal element is less than 5 ppb, the synthetic quartz has a more excellent transmittance in the ultraviolet band and the vacuum ultraviolet band, and has lower stress birefringence and optical inhomogeneity in the ultraviolet band and the vacuum ultraviolet band.
[0083] A second aspect of the present invention provides a method for preparing the above-mentioned synthetic quartz, which comprises the following steps:
[0084] Performing a deposition process on the silicon-containing raw material to obtain a silicon dioxide preform;
[0085] The silicon dioxide preform is sequentially subjected to dehydroxylation treatment, inert gas replacement treatment, oxidation treatment, sintering treatment, annealing treatment and hydrogen gas treatment to obtain synthetic quartz;
[0086] The present invention does not specifically limit the silicon source, and a silicon source commonly used in the art can be selected. In some embodiments, the silicon source can be selected from silicon tetrachloride and / or octamethylcyclotetrasiloxane. In the present invention, the hydrogen-based gas can be selected from hydrogen and / or deuterium.
[0087] Specifically, the preparation method of the present invention comprises: hydrolyzing a silicon source into silicon dioxide at high temperature under the action of a combustion gas, and depositing the silicon dioxide on a target carrier, and removing the target carrier to obtain a silicon dioxide preform;
[0088] The silicon dioxide preform is subjected to a dehydroxylation treatment in a vacuum or a halogen-containing gas to remove hydroxyl groups in the silicon dioxide preform. When the silicon source contains halogen elements, the dehydroxylation treatment can also remove halogen-containing compounds in the silicon dioxide preform, thereby obtaining a dehydroxylation preform with less hydroxyl content and less halogen elements. The dehydroxylation preform with less halogen elements is not easy to generate ≡Si-X (X is a halogen element) in the subsequent sintering treatment, which helps to improve the transmittance of synthetic quartz;
[0089] Using an inert gas to perform an inert gas replacement treatment on the dehydroxylated preform to reduce the content of halogen elements in the dehydroxylated preform to obtain a replacement preform;
[0090] performing oxidation treatment on the replacement preform to eliminate oxygen defects in the replacement preform to obtain an oxidized preform;
[0091] Sintering the oxide preform to vitrify the oxide preform to form a synthetic quartz body;
[0092] Annealing the synthetic quartz body to eliminate the internal stress of the synthetic quartz body so as to improve the mechanical properties of the synthetic quartz body and obtain an annealed body;
[0093] The annealed body is subjected to gas treatment using a hydrogen-based gas so that hydrogen molecules and / or deuterium molecules are contained in the annealed body, thereby obtaining synthetic quartz.
[0094] In some embodiments, the deposition process may be performed in a deposition chamber, which may be made of high-purity synthetic quartz, and the inner wall of the deposition chamber needs to be cleaned and baked before each deposition process.
[0095] In the present invention, when the dehydroxylation atmosphere is a gas containing halogen elements, the concentration of the gas containing halogen elements is 99.9999% or more. The present invention does not particularly limit the gas containing halogen elements, and the gas containing halogen elements can be at least one of chlorine-containing gas, bromine-containing gas and fluorine-containing gas. In a specific embodiment, when the dehydroxylation atmosphere is a fluorine-containing gas, the effect of the dehydroxylation treatment can be further improved, thereby improving the transmittance of synthetic quartz. When the dehydroxylation atmosphere is a fluorine-containing gas, the fluorine-containing gas can be selected from at least one of fluorine gas (F2), silicon tetrafluoride (SiF4) and sulfur hexafluoride (SF6).
[0096] The present invention can prepare synthetic quartz with excellent transmittance, excellent optical non-uniformity and low stress in the ultraviolet band and vacuum ultraviolet band through the preparation method, and the preparation method has a simple preparation process and is suitable for wide promotion and application.
[0097] In some embodiments of the present invention, the process parameters in the deposition process can be specifically selected. When the temperature is 1000-1200° C. and the pressure is -80 to -20 Pa during the deposition process, a high-purity and high-uniformity silicon dioxide preform can be obtained.
[0098] In some embodiments of the present invention, when the combustion gas includes hydrogen and oxygen in the deposition process, and the equivalent volume ratio of hydrogen and oxygen in the combustion gas is (2.1-2.8):1, the silicon source can be hydrolyzed into more silicon dioxide while saving combustion gas, thereby improving the efficiency of the deposition process.
[0099] In some embodiments of the present invention, when the temperature is 1100-1300° C. and the time is 4-40 in the dehydroxylation treatment, the hydroxyl groups and chlorine-containing compounds in the silica preform can be better removed, thereby improving the transmittance of the synthetic quartz.
[0100] In the present invention, the process parameters in the inert gas replacement treatment can also be selected to better remove the halogen elements in the dehydroxylated preform and improve the transmittance of the synthetic quartz. In some embodiments of the present invention, in the inert gas replacement treatment, the pressure is 100-10000 Pa, the time is 1-10 hours, and the temperature is 1100-1300°C.
[0101] In some embodiments of the present invention, the oxidation treatment includes soaking the replacement preform in a dry oxygen-rich environment to eliminate oxygen defects in the soaking pretreatment. When the oxidation treatment is carried out at a temperature of 1000-1400°C, an oxygen partial pressure of 100-10000Pa, a mass percentage of water in oxygen of less than 1ppm, and a time of 1-5 hours, oxygen defects in the replacement preform can be better eliminated, which helps to prevent the transmittance of the synthetic quartz from decaying too quickly.
[0102] In the present invention, the atmosphere of the oxygen-rich environment can be selected from at least one of oxygen, dry air and laughing gas (N2O).
[0103] In the present invention, the oxide preform obtained after the oxidation treatment can be placed in a vacuum sintering furnace for sintering treatment. The vacuum degree and the temperature rise slope of the sintering furnace can be further controlled to prevent microscopic defects from being generated inside the oxide preform during the sintering process. In some embodiments of the present invention, the sintering treatment includes:
[0104] Under a vacuum degree of ≤10Pa, heating the oxidized silicon dioxide preform from 0°C to 1000°C at a rate of 100-500°C / h to obtain a first sintered preform;
[0105] Under a vacuum degree of ≤5 Pa, heating the first sintered preform from 1000° C. to 1300° C. at a rate of 2-5° C. / h to obtain a second sintered preform;
[0106] Under a vacuum degree of ≤2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 6-10° C. / h to obtain a third sintered preform;
[0107] The third sintered preform is sintered at a vacuum degree of ≤1 Pa and a temperature of 1500° C. for 1-2 hours to obtain a synthetic quartz body.
[0108] The present invention controls the heating rate during the sintering process, which can not only make the oxidized preform shrink uniformly due to heat to obtain a synthetic quartz blank with uniform density, but also can slowly discharge the gas generated by the oxidized preform during the sintering process out of the sintering furnace, thereby more stably controlling the vacuum degree of the sintering furnace and improving safety performance.
[0109] In some embodiments of the present invention, the annealing process can be further selected to better reduce the internal stress in the synthetic quartz body and improve the mechanical properties of the synthetic quartz. The annealing process includes: heat preservation treatment of the synthetic quartz body at 1050°C-1300°C, cooling treatment to 800-900°C at a cooling rate of less than or equal to 2°C / h, and naturally cooling to room temperature.
[0110] It can be understood that the present invention can place the synthetic quartz blank in an annealing furnace, use a temperature of 1050-1300°C to keep the synthetic quartz blank warm, then cool it at a cooling rate of less than or equal to 2°C / h until the temperature is 800-900°C, and finally close the annealing furnace to allow the synthetic quartz blank to cool naturally to room temperature to obtain an annealed blank.
[0111] The present invention can further select the process parameters of hydrogen gas treatment to improve the effect of hydrogen gas treatment and the transmittance of synthetic quartz. In some embodiments of the present invention, in hydrogen gas treatment, the volume percentage of hydrogen gas is 5-100%, the temperature is 300-500°C, the pressure is 0.1-1MPa, and the time is 5-100h.
[0112] Specifically, the annealing body is placed in a gas carrier furnace, hydrogen-based gas of the above concentration is introduced into the gas carrier furnace, the furnace temperature is controlled at 300-500° C., the pressure is 0.1-1 MPa, and maintained for 5-100 hours, so that the hydrogen-based gas penetrates into the interior of the annealing body, thereby obtaining synthetic quartz containing hydrogen molecules and / or deuterium molecules.
[0113] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0114] Example 1
[0115] The synthetic quartz in this embodiment is prepared by a method comprising the following steps:
[0116] 1) Under the action of combustion gas, a silicon source is deposited to convert the silicon source into silicon dioxide and deposit it on a target carrier, and the target carrier is removed to obtain a silicon dioxide preform;
[0117] The silicon source is silicon tetrachloride, the temperature is 1050°C, and the pressure is -30Pa;
[0118] The combustion gas includes hydrogen and oxygen, and the equivalent volume ratio of hydrogen to oxygen in the combustion gas is 2.1:1;
[0119] 2) dehydroxylating the silicon dioxide preform in a mixed gas of chlorine and silicon tetrafluoride (the volume percentage of silicon tetrafluoride is 20%) to obtain a dehydroxylated preform;
[0120] Among them, the temperature is 1100°C and the time is 5 hours;
[0121] 3) using an inert gas to perform an inert gas replacement treatment on the dehydroxylated preform to obtain a replacement preform;
[0122] The inert gas is nitrogen, the pressure is 500 Pa, the time is 2 hours, and the temperature is 1100°C;
[0123] 4) performing oxidation treatment on the replacement preform to obtain an oxidized preform;
[0124] Among them, the oxygen partial pressure is 1000Pa, the temperature is 1000 degrees Celsius, the mass percentage of water in oxygen is 1ppm, and the time is 1 hour;
[0125] 5) Sintering the oxide preform to form a synthetic quartz body, the sintering process sequentially comprising:
[0126] Under a vacuum degree of 8 Pa, heating the oxidation preform from 0° C. to 1000° C. at a rate of 150° C. / h to obtain a first sintered preform;
[0127] Under a vacuum degree of 2 Pa, heating the first sintered preform from 1000° C. to 1300° C. at a rate of 5° C. / h to obtain a second sintered preform;
[0128] Under a vacuum degree of 2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 10° C. / h to obtain a third sintered preform;
[0129] The third sintered preform is sintered at a vacuum degree of 1 Pa and a temperature of 1500° C. for 1 hour to obtain a synthetic quartz body;
[0130] 6) Annealing the synthetic quartz body to obtain an annealed body. The annealing temperature and the cooling rate are shown in Table 1;
[0131] 7) using hydrogen to treat the annealed body with hydrogen to obtain synthetic quartz;
[0132] The volume percentage of hydrogen is 10%, the temperature is 350° C., the pressure is 0.1 MPa, and the time is 10 h.
[0133] Example 2
[0134] The preparation method of synthetic quartz in this embodiment is basically the same as the preparation method of synthetic quartz in Example 1, except that:
[0135] In step 1), the temperature is 1070°C and the pressure is -35Pa;
[0136] The equivalent volume ratio of hydrogen to oxygen in the combustion gas is 2.1:1.
[0137] In step 2), the volume percentage of silicon tetrafluoride in the mixed gas of chlorine and silicon tetrafluoride is 18%;
[0138] In step 3), the pressure is 100 Pa and the time is 4 hours;
[0139] In step 4), the time is 2 hours;
[0140] In step 5), under a vacuum degree of 2 Pa, the first sintered preform is heated from 1000° C. to 1300° C. at a rate of 4° C. / h to obtain a second sintered preform;
[0141] Under a vacuum degree of 2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 8° C. / h to obtain a third sintered preform;
[0142] In step 7), the volume percentage of hydrogen is 15% and the pressure is 0.2 MPa.
[0143] Example 3
[0144] The preparation method of synthetic quartz in this embodiment is basically the same as the preparation method of synthetic quartz in Example 1, except that:
[0145] In step 1), the temperature is 1100°C and the pressure is -40Pa; the equivalent volume ratio of hydrogen to oxygen in the combustion gas is 2.4:1;
[0146] In step 2), the volume percentage of silicon tetrafluoride in the mixed gas of chlorine and silicon tetrafluoride is 15%;
[0147] In step 3), the pressure is 1000 Pa and the time is 5 hours;
[0148] In step 4), the time is 3 hours;
[0149] In step 5), under a vacuum degree of 2 Pa, the first sintered preform is heated from 1000° C. to 1300° C. at a rate of 3° C. / h to obtain a second sintered preform;
[0150] Under a vacuum degree of 2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 7° C. / h to obtain a third sintered preform;
[0151] In step 7), the volume percentage of hydrogen is 25% and the pressure is 0.3 MPa.
[0152] Example 4
[0153] The preparation method of synthetic quartz in this embodiment is basically the same as the preparation method of synthetic quartz in Example 1, except that:
[0154] In step 1), the temperature is 1100°C and the pressure is -45Pa; the equivalent volume ratio of hydrogen to oxygen in the combustion gas is 2.6:1;
[0155] In step 2), the volume percentage of silicon tetrafluoride in the mixed gas of chlorine and silicon tetrafluoride is 10%; the time is 10 hours;
[0156] In step 3), the inert gas is a mixture of argon and helium, the volume percentage of helium in the mixture of argon and helium is 10%, the pressure is 5000 Pa, and the time is 8 hours;
[0157] In step 4), the oxygen partial pressure is 3000 Pa and the time is 5 hours;
[0158] In step 5), under a vacuum degree of 2 Pa, the first sintered preform is heated from 1000° C. to 1300° C. at a rate of 2° C. / h to obtain a second sintered preform;
[0159] Under a vacuum degree of 2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 5° C. / h to obtain a third sintered preform;
[0160] In step 7), the volume percentage of hydrogen is 50%, the temperature is 400° C., and the pressure is 0.5 MPa.
[0161] Example 5
[0162] The preparation method of synthetic quartz in this embodiment is basically the same as the preparation method of synthetic quartz in Example 1, except that:
[0163] In step 1), the silicon source is octamethylcyclotetrasiloxane;
[0164] In step 2), the volume percentage of silicon tetrafluoride in the mixed gas of chlorine and silicon tetrafluoride is 10%, and the time is 10 hours;
[0165] In step 3), the inert gas is a mixture of argon and helium, the volume percentage of helium in the mixture of argon and helium is 20%, the pressure is 5000 Pa, and the time is 8 hours;
[0166] In step 4), the oxygen partial pressure is 3000 Pa and the time is 5 hours;
[0167] In step 5), under a vacuum degree of 2 Pa, the first sintered preform is heated from 1000° C. to 1300° C. at a rate of 2° C. / h to obtain a second sintered preform;
[0168] Under a vacuum degree of 2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 5° C. / h to obtain a third sintered preform;
[0169] In step 7), the volume percentage of hydrogen is 50%, the temperature is 300° C., and the time is 5 hours.
[0170] Example 6
[0171] The preparation method of synthetic quartz in this embodiment is basically the same as the preparation method of synthetic quartz in Example 1, except that:
[0172] In step 1), the silicon source is octamethylcyclotetrasiloxane;
[0173] In step 2), the volume percentage of silicon tetrafluoride in the mixed gas of chlorine and silicon tetrafluoride is 10%, and the time is 20 hours;
[0174] In step 3), the inert gas is a mixture of argon and helium, the volume percentage of helium in the mixture is 20%, the pressure is 10000 Pa, and the time is 10 hours;
[0175] In step 4), the oxygen partial pressure is 3000 Pa and the time is 5 hours;
[0176] In step 5), under a vacuum degree of 2 Pa, the first sintered preform is heated from 1000° C. to 1300° C. at a rate of 2° C. / h to obtain a second sintered preform;
[0177] Under a vacuum degree of 2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 5° C. / h to obtain a third sintered preform;
[0178] In step 7), the volume percentage of hydrogen is 20%, the temperature is 300° C., the pressure is 0.1 MPa, and the time is 5 hours.
[0179] Comparative Example 1
[0180] The preparation method of the synthetic quartz in this comparative example is basically the same as the preparation method of the synthetic quartz in Example 1, except that:
[0181] In step 1), the temperature is 1100° C.;
[0182] In step 2), the silicon dioxide preform is subjected to a dehydroxylation treatment in chlorine gas to obtain a dehydroxylated preform;
[0183] Without performing step 3), the dehydroxylated preform is directly subjected to oxidation treatment to obtain an oxidized preform.
[0184] Performance Testing
[0185] The following tests were performed on the synthetic quartz in the embodiments and comparative examples, and the test results are shown in Table 1;
[0186] 1. Composition of synthetic quartz
[0187] 1) Mass percentage of silicon dioxide
[0188] The mass percentage of silicon dioxide in synthetic quartz was determined using the loss on ignition method described in GB / T 3284-2015 Chemical analysis method for synthetic quartz composition.
[0189] 2) Mass percentage of -OH
[0190] The mass percentage of -OH in synthetic quartz was determined using a spectrophotometer as described in GB / T 12442-2019 Test method for hydroxyl content in synthetic quartz.
[0191] 3) Chlorine and fluorine content
[0192] The X-ray fluorescence spectrometry in GB / T 176-2017 cement chemical analysis method was used to test the chlorine and fluorine contents in synthetic quartz.
[0193] 4) Hydrogen and deuterium content
[0194] The Raman spectroscopic method disclosed in "Determining the content of hydrogen dissolved in quartz glassusing the methods of roman scattering and mass spectrometry", Khotimchenko, is used to determine the content of hydrogen and tritium in synthetic quartz, specifically including:
[0195] The molecular concentration of hydrogen and deuterium in synthetic quartz can be expressed as:
[0196]
[0197] in, Peak value 800cm -1 The Raman intensity at The peak value is 4135cm -1 The Raman intensity at .
[0198] 5) Oxygen vacancy defect content, peroxide defect content and SiH content
[0199] By "Reaction of hydrogen with hydroxyl-free vitreous silica",
[0200] The Shelby method described in J. Appl. Phys., Vol. 51, No. 5 (May 1980), pp. 2589-2593, is used to determine the content of oxygen vacancy defects, the content of peroxygen defects, and the content of SiH in synthetic quartz.
[0201] 6) Alkali metal content, alkaline earth metal content and transition metal content
[0202] The content of alkali metal elements, alkaline earth metal elements and transition metal elements in synthetic quartz was determined by inductively coupled plasma mass spectrometry as recorded in GB / T 32650-2016 Inductively coupled plasma mass spectrometry for detecting trace elements in quartz sand.
[0203] 2. Properties of synthetic quartz
[0204] 1) 633nm stress birefringence
[0205] The stress birefringence of synthetic quartz was measured using a high-precision stress birefringence instrument from German Ilis Company, including:
[0206] The natural light emitted by the light source passes through the polarizer to produce linear polarized light. The linear polarized light passes through synthetic quartz. Due to the birefringence effect, the linear polarized light becomes elliptically polarized light after passing through synthetic quartz. It then passes through a quarter-wave plate to become linear polarized light. Finally, the analyzer is rotated to obtain a new extinction position. The deflection angle of the analyzer is recorded. The stress birefringence is determined based on the deflection angle. The relationship between the deflection angle ɑ and the optical path difference Δ is:
[0207]
[0208] 2) Optical inhomogeneity
[0209] The optical inhomogeneity of synthetic quartz was tested using the method in JC / T 185-2013 Optical Synthetic Quartz, and was specifically measured using an American 4D AcuuFiz laser interferometer.
[0210] 3) Initial internal transmittance and irradiated internal transmittance
[0211] Initial internal transmittance refers to the internal transmittance of the original synthetic quartz to the laser in this band, and irradiated internal transmittance refers to the internal transmittance of the laser when the energy is 10mJ / cm 2 , the pulse is 2×10 6 Internal transmittance of synthetic quartz after irradiation with light;
[0212] The internal transmittance (including the initial internal transmittance and the irradiated internal transmittance) is obtained by correcting the external transmittance for reflection loss. The external transmittance is measured using an American vacuum ultraviolet spectrophotometer. The internal transmittance is obtained using the following formula:
[0213]
[0214]
[0215] Among them, n λT is the refractive index of synthetic quartz to light of wavelength λ; theroy is the theoretical transmittance; T e is the external transmittance of synthetic quartz at wavelength λ; T i It is the internal transmittance of synthetic quartz at wavelength λ.
[0216] Table 1
[0217]
[0218]
[0219] It can be seen from Table 1 that the synthetic quartz in the embodiment of the present invention has excellent transmittance in the ultraviolet band, and has relatively low stress birefringence and optical inhomogeneity.
[0220] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A synthetic quartz, characterized in that: The stress birefringence of the synthetic quartz to light with a wavelength of 633 nm is ≤1.6 nm / cm, and the optical inhomogeneity to light with a wavelength of 633 nm is ≤2.1×10 -6 ; The synthetic quartz having a thickness of 10 mm has an initial internal transmittance of ≥99.6% for light having a wavelength of 193 nm, and an initial internal transmittance of ≥88.3% for light having a wavelength of 157 nm.
2. The synthetic quartz according to claim 1, characterized in that The synthetic quartz with a thickness of 10 mm has a wavelength of 193 nm and an energy of 10 mJ / cm 2 , the pulse is 2×10 6 After light irradiation, the internal transmittance decreases by ≤0.6%.
3. The synthetic quartz according to claim 1 or 2, characterized in that: In the synthetic quartz, The mass percentage of SiO2 is greater than 99.999%; The mass percentage of hydroxyl is 0.1-50ppm; The mass percentage of chlorine element is less than 10ppm; The content of fluorine is 0.1-2 mol / cm 3 ; The sum of the contents of hydrogen and deuterium is 1×10 15 -2×10 18 molecules / cm 3 ; The content of silicon-hydrogen bonds is less than 2×10 17 Pieces / cm 3 ; The content of oxygen vacancies is less than 1×10 16 Pieces / cm 3 ; The content of peroxygen defects is less than 1×10 16 Pieces / cm 3 ; The mass percentage of alkali metal elements is less than 20ppb; The mass percentage of alkaline earth metal elements is less than 10ppb; The mass percentage of transition metal elements is less than 20ppb.
4. The synthetic quartz according to claim 3, characterized in that In the synthetic quartz, The mass percentage of SiO2 is greater than 99.9997%; The mass percentage of hydroxyl is 10-30ppm; The mass percentage of chlorine element is less than 2ppm; The content of fluorine is 0.6-1 mol / cm 3 ; The sum of the contents of hydrogen and deuterium is 2×10 16 -2×10 17 molecules / cm 3 ; The content of silicon-hydrogen bonds is less than 1×10 16 molecules / cm 3 ; The content of oxygen vacancies is less than 1×10 15 Pieces / cm 3 ; The content of peroxygen defects is less than 1×10 15 Pieces / cm 3 ; The mass percentage of alkali metal elements is less than 5ppb; The mass percentage of alkaline earth metal elements is less than 2ppb; The mass percentage of transition metal elements is less than 5ppb.
5. A method for preparing synthetic quartz according to any one of claims 1 to 4, characterized in that: The following steps are involved: Performing deposition treatment on a silicon source to obtain a silicon dioxide preform; The synthetic quartz is obtained by sequentially subjecting the silicon dioxide preform to dehydroxylation treatment, inert gas replacement treatment, oxidation treatment, sintering treatment, annealing treatment and hydrogen-based gas treatment.
6. The preparation method according to claim 5, characterized in that: During the deposition process, the temperature is 1000-1200° C. and the pressure is -80 to -20 Pa; and / or, In the deposition process, the combustion gas includes hydrogen and oxygen, and the equivalent volume ratio of hydrogen to oxygen in the combustion gas is (2.1-2.8):1; and / or, In the dehydroxylation treatment, the temperature is 1100-1300° C. and the time is 4-40 hours.
7. The preparation method according to claim 5 or 6, characterized in that: In the inert gas replacement treatment, the pressure is 100-10000 Pa, the time is 1-10 hours, and the temperature is 1100-1300° C.; and / or, In the oxidation treatment, the temperature is 1000-1400° C., the oxygen partial pressure is 100-10000 Pa, the mass percentage of water in the oxygen is less than 1 ppm, and the time is 1-5 hours.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The sintering process comprises in sequence: Under a vacuum degree of ≤10 Pa, heating the oxidized silicon dioxide preform from 0° C. to 1000° C. at a rate of 100-500° C. / h to obtain a first sintered preform; Under a vacuum degree of ≤5 Pa, heating the first sintered preform from 1000° C. to 1300° C. at a rate of 2-5° C. / h to obtain a second sintered preform; Under a vacuum degree of ≤2 Pa, heating the second sintered preform from 1300° C. to 1500° C. at a rate of 6-10° C. / h to obtain a third sintered preform; The third sintered preform is sintered at a vacuum degree of ≤1 Pa and a temperature of 1500° C. for 1-2 hours to obtain a synthetic quartz blank.
9. The preparation method according to claim 8, characterized in that: The annealing treatment includes: heat-insulating the synthetic quartz blank at 1050° C.-1300° C., cooling the blank to 800-900° C. at a cooling rate of less than or equal to 2° C. / h, and naturally cooling the blank to room temperature.
10. The preparation method according to any one of claims 5 to 9, characterized in that: In the hydrogen-based gas treatment, the volume percentage of the hydrogen-based gas is 5-100%, the temperature is 300-500° C., the pressure is 0.1-1 MPa, and the time is 5-100 h.