Flue gas circulation system and method for sintering CO-NOx synergistic removal and energy-saving optimization

By using sinter and calcium ferrite components to perform high-temperature catalytic oxidation and reduction in the sintering flue gas circulation system, combined with SCR deep denitrification and waste heat utilization, the problem of insufficient CO and NOx emission reduction effects in the existing technology is solved, and the Efficient pollutant absorption and energy efficiency improvement.

CN118856907APending Publication Date: 2024-10-29SHOUGANG QIANAN IRON & STEEL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410812375.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing sintering flue gas circulation technology has insufficient CO and NOx emission reduction effects, and the purification mechanism is unclear, resulting in no significant reduction in total pollutant emissions. The desulfurization process has high load and cost, and the desulfurization agent utilization rate is low, resulting in the production of a large amount of desulfurization ash. .

Method used

A sintered CO-NOx collaborative removal and energy-saving optimized flue gas circulation system is designed. By using sinter and calcium ferrite components in the ring cooling module for high-temperature catalytic oxidation and reduction, combined with SCR deep denitrification and waste heat utilization, Optimize the distribution and temperature characteristics of flue gas components to achieve coordinated CO-NOx removal and waste heat recovery.

Benefits of technology

It achieves efficient coordinated consumption of CO-NOx, reduces CO and NOx pollution emissions from the sintering process in the steel production process, improves energy efficiency, reduces flue gas treatment load and energy consumption, and reduces comprehensive carbon emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118856907A_ABST
    Figure CN118856907A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flue gas treatment, and discloses a sintering CO-NOx collaborative removal and energy-saving optimization flue gas circulation system and method, the sintering CO-NOx collaborative removal and energy-saving optimization flue gas circulation system comprises a sintering module A, an air bellow group and a ring cooling module B, and is characterized by comprising five flue gas channels, three gas distribution channels and a purified gas channel, the air bellow set is provided with an air inducing area C, an air inducing area D, an air inducing area E and an air inducing area F, the flue gas channel i is used for conveying CO-NOx treated flue gas, the flue gas channel ii is used for conveying high-sulfur CO-NOx treated flue gas, the flue gas channel iii is used for conveying oxygen-enhanced flue gas, the flue gas channel iv is used for conveying NOx treated gas, the flue gas channel v is used for CO treated gas, and the flue gas channel i is used for conveying high-oxygen distributed gas; the construction of a flue gas circulation system for efficient and collaborative absorption of CO and NOx and multi-efficiency improvement in the sintering-circular cooling process is realized, so that the pollutant emission of high-proportion CO and NOx in the sintering process in the whole steel process is reduced, and the energy efficiency of the sintering-circular cooling process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flue gas treatment, and in particular to a flue gas circulation system and method for sintering CO-NOx synergistic removal and energy-saving optimization. Background Art

[0002] Sintering flue gas circulation technology is a method for improving the sintering process by actively returning part of the heat-carrying flue gas generated during the sintering process to the upper part of the sintering material surface and allowing it to re-participate in the sintering process. This type of technology can realize the recycling of waste heat from hot flue gas, and absorb pollutants such as CO and NOx in part of the circulating flue gas, thereby reducing the total amount of pollutant emissions. However, the current effect of reducing CO and NOx emissions mainly comes from the reduction in the total amount of flue gas generated by the flue gas circulation process. The actual reduction in pollutant concentration is insufficient, and there are still problems such as unclear purification mechanisms, insignificant emission reduction effects, or even increases instead of decreases. At present, the denitrification, deCO and waste heat utilization technologies related to the sintering process are all operated independently, and the flue gas allocation within the process is relatively simple. In addition, most of the purification treatment technologies such as denitrification and deCO require additional control of the components or the addition of independent treatment devices. The additional input for the target is large and the operating cost is high. In addition, the current main technology for sintering flue gas desulfurization treats the mixed flue gas of the whole bellows, with low SO2 concentration and large flue gas treatment volume, which makes the flue gas load of the desulfurization process high, the utilization rate of the desulfurizer is low, the dosage is large and leads to the generation of a large amount of desulfurization ash. Summary of the invention

[0003] The object of the present invention is to provide a flue gas circulation system and method for sintering CO-NOx coordinated removal and energy saving optimization, so as to solve the problems raised in the above background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] The flue gas circulation system for sintering CO-NOx synergistic removal and energy-saving optimization includes a sintering module A, a wind box group and an annular cooling module B, and is characterized in that: it includes five flue gas channels, three gas distribution channels and one purified gas channel, and the wind box group has an induced draft area C, an induced draft area D, an induced draft area E, and an induced draft area F;

[0006] The flue gas i channel is formed by the induced draft area D and the first gas mixing unit (3) and the electrostatic precipitator unit (4) being connected in one direction in sequence through pipelines. The flue gas i channel is used to transport CO-NOx treated flue gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is less than 50mg / Nm 3 , the flue gas temperature is higher than 200℃;

[0007] The flue gas ii channel is formed by the induced draft area E and the desulfurization unit (1), the dust removal unit (2), and the first gas mixing unit (3) being connected in one direction in sequence through pipelines. The flue gas ii channel is used to transport high-sulfur CO-NOx treated flue gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is higher than 50mg / Nm 3 ;

[0008] The flue gas iii channel is formed by the induced draft area F and the oxygen-raising gas mixing unit (6) being connected in one direction. The flue gas iii channel is used to transport oxygen-raising flue gas, specifically, the oxygen content is higher than 16%, and the SO2 concentration is higher than 50mg / Nm 3 , the flue gas temperature is higher than 500℃;

[0009] The flue gas IV channel is formed by the electrostatic precipitator unit (4) sequentially connected in one direction in series with the NOx treatment unit (5) and the oxygen supply and mixing unit (6); the NOx treatment unit (5) is arranged in the ring cooling section II-ring cooling section III of the ring cooling module B; the flue gas IV channel is used to transport the NOx treated gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is less than 50mg / Nm 3 , the flue gas temperature is higher than 150℃;

[0010] The flue gas v channel is formed by the one-way connection between the oxygen supply and gas mixing unit (6) and the CO processing unit (7). The flue gas v channel is used for CO processing gas, specifically, the CO:O2 volume concentration ratio is less than 0.5, and the SO2 concentration is lower than 35 mg / Nm 3 , the flue gas temperature is higher than 500℃;

[0011] The CO treatment unit (7) is respectively connected to the SCR deep denitration unit (9) and the gas distribution unit (8) to form a gas distribution channel ii and a gas distribution channel iii;

[0012] The air distribution channel i is formed by the unidirectional communication between the air induction area C and the air distribution unit (8), and is used to transport high-oxygen distribution air, specifically, an oxygen content higher than 16%;

[0013] The SCR deep denitration unit (9), the waste heat utilization unit (10), and the chimney are connected in series and one-way to form a purified gas channel.

[0014] As a further solution of the present invention: the oxygen content of the distribution gas iii after being treated by the distribution unit is greater than 18%.

[0015] As a further solution of the present invention: the treatment temperature of the NOx treatment unit is 400-600°C, and the reaction time is greater than 600s.

[0016] As a further solution of the present invention: the processing temperature of the CO processing unit is 600-800° C., and the reaction time is 30-60 s.

[0017] As a further solution of the present invention, a method for using a flue gas circulation system for sintering CO-NOx synergistic removal and energy saving optimization includes:

[0018] A: Based on the temperature of the sintered hot ore from high to low and the transportation direction during the ring cooling process, the ring cooling section is divided into the ring cooling section I-ring cooling section V. After the flue gas II passes through the desulfurization unit and the dust removal unit, it is mixed with the flue gas I in the first gas mixing unit and enters the electrostatic precipitator unit. After mixing, it enters the NOx treatment unit as flue gas iv, and uses a gas-solid countercurrent method to sequentially contact with the high-temperature sintered hot ore in the ring cooling section III and the ring cooling section II for heating and calcium ferrite catalysis. After CO-NOx synergistic NOx reduction, the flue gas iv enters the oxygen extraction and gas mixing unit and mixes with the flue gas III to extract oxygen. After mixing, it enters the CO treatment unit as flue gas V, and uses a gas-solid countercurrent method to oxidize CO and release heat and remove CO with the high-temperature sintered hot ore in the ring cooling section I. After CO oxidation heat release and sintering hot ore waste heat recovery, the gas is used as distribution gas II, and then enters the distribution unit according to the sintering distribution gas and oxygen content control, mixed with distribution gas I and introduced into natural air to adjust the air volume and oxygen content, and then used as distribution gas III to supply the sintering process after adjustment. The remaining distribution gas II enters the SCR deep denitrification unit, and after deep denitrification, it enters the waste heat utilization unit as purified gas for waste heat utilization, and then is discharged from the chimney in the factory.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The high-temperature sintered ore and calcium ferrite components contained in the ring cooling section of the sintering process are used to carry out the synergistic catalysis and CO-O2 catalytic oxidation of high-concentration CO and NOx generated by the sintering flue gas in the ring cooling section. In order to achieve the synergistic removal of CO-NOx in the production process, improve the utilization of waste heat and reduce the load of flue gas pollutant treatment, by studying the emission components and temperature characteristics of flue gas at each stage of sintering process, the synergistic catalytic purification mechanism of CO-NOx catalyzed by sintered ore and calcium ferrite and the optimization of process parameters, combined with the selection and allocation parameters and scheme design of flue gas in the sintering-ring cooling process. Achieve the construction of a flue gas circulation system with efficient synergistic absorption of CO and NOx and multi-efficiency improvement in the sintering-ring cooling process, so as to reduce the high proportion of CO and NOx pollution emissions in the sintering process in the entire steel process, and improve the energy efficiency of the sintering-ring cooling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0022] Figure 1 Schematic diagram of flue gas circulation system optimized for sintering CO-NOx synergistic removal and energy saving;

[0023] Figure 2 This is a schematic diagram comparing the catalytic oxidation effects of CF and SO2 on CO;

[0024] Figure 3 This is the CO oxidation efficiency diagram catalyzed by calcium ferrite sinter with different oxygen contents;

[0025] Figure 4 This is the conversion efficiency diagram of NOx by calcium ferrite sintered ore under low oxygen conditions;

[0026] Figure 5 Schematic diagram of the effect of CF on SO2 absorption and NOx conversion;

[0027] In the figure: 1. Desulfurization unit; 2. Dust removal unit; 3. First gas mixing unit; 4. Electrostatic precipitator unit; 5. NOx treatment unit; 6. Oxygen mixing unit; 7. CO treatment unit; 8. Gas distribution unit; 9. SCR deep denitrification unit; 10. Waste heat utilization unit. DETAILED DESCRIPTION

[0028] See also Figure 1-Figure 5 :

[0029] In this embodiment, a sintering module A, a wind box group and an annular cooling module B are included, and the features include: five flue gas channels, three gas distribution channels and one purified gas channel, and the wind box group has an induced draft area C, an induced draft area D, an induced draft area E and an induced draft area F;

[0030] The flue gas i channel is formed by the induced draft area D and the first gas mixing unit (3) and the electrostatic precipitator unit (4) being connected in one direction in sequence through pipelines. The flue gas i channel is used to transport CO-NOx treated flue gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is less than 50mg / Nm 3 , the flue gas temperature is higher than 200℃;

[0031] The flue gas ii channel is formed by the induced draft area E and the desulfurization unit (1), the dust removal unit (2), and the first gas mixing unit (3) being connected in one direction in sequence through pipelines. The flue gas ii channel is used to transport high-sulfur CO-NOx treated flue gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is higher than 50mg / Nm 3 ;

[0032] The flue gas iii channel is formed by the induced draft area F and the oxygen-raising gas mixing unit (6) being connected in one direction. The flue gas iii channel is used to transport oxygen-raising flue gas, specifically, the oxygen content is higher than 16%, and the SO2 concentration is higher than 50mg / Nm 3 , the flue gas temperature is higher than 500℃;

[0033] The flue gas iv channel is formed by the electrostatic precipitator unit (4) sequentially connected in series with the NOx treatment unit (5) and the oxygen extraction and mixing unit (6) in one direction. The NOx treatment unit (5) is arranged in the ring cooling section II-ring cooling section III of the ring cooling module B. The flue gas iv channel is used to transport the NOx treated gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50mg / Nm 3 , SO2 concentration is less than 50mg / Nm 3 , the flue gas temperature is higher than 150℃;

[0034] The flue gas v channel is formed by the one-way connection between the oxygen supply and mixing unit (6) and the CO treatment unit (7). The flue gas v channel is used for CO treatment gas, specifically, the CO:O2 volume concentration ratio is less than 0.5, and the SO2 concentration is lower than 35 mg / Nm 3 , the flue gas temperature is higher than 500℃;

[0035] The CO treatment unit (7) is respectively connected with the SCR deep denitration unit (9) and the gas distribution unit (8) to form a gas distribution channel ii and a gas distribution channel iii;

[0036] The air distribution channel i is formed by the unidirectional connection between the air induction area C and the air distribution unit (8), and is used to transport high-oxygen distribution air, specifically, an oxygen content higher than 16%;

[0037] The SCR deep denitration unit (9), the waste heat utilization unit (10), and the chimney are connected in series and one-way to form a purified gas channel.

[0038] In this embodiment, please refer to Figure 2 , using the waste heat of sintering ring cooling and the strong catalytic oxidation ability of calcium ferrite (CF) contained in sintering ore to CO, catalytic oxidation of high-concentration CO in sintering flue gas is released. The catalytic oxidation effect of calcium ferrite component of sintering ore on CO at different temperatures is shown in the figure. Figure 2As shown, more than 65% of CO catalytic oxidation can be achieved at 600°C, and more than 95% of catalytic oxidation efficiency can be achieved at 800°C. Compared with the SiO2 control group with no catalytic effect, the catalytic oxidation efficiency of calcium ferrite for CO above 600°C is increased by more than 6 times. Based on the test results, the catalytic oxidation ability of calcium ferrite components in sintered ore for CO can be used to improve the utilization efficiency of sintering flue gas waste heat, reduce the dissipation of waste heat in the form of chemical energy and environmental pollutant emissions in the sintering process, and reduce the comprehensive carbon emissions of the sintering process.

[0039] In this embodiment, please refer to Figure 3 , the effect of flue gas oxygen content at 600℃ was tested, such as Figure 3 As shown. It shows that the catalytic effect of sintered calcium ferrite on CO at an oxygen content of 5% has a CO catalytic purification efficiency close to the highest catalytic efficiency at this temperature.

[0040] In this embodiment, please refer to Figure 4 The high concentration of CO in sintering flue gas and the calcium ferrite component of sintered ore are used to efficiently catalyze and reduce the NOx contained in the same flue gas. The catalytic reduction effect of NOx is as follows: Figure 4 As shown, the catalytic reaction is based on the ER mechanism. O2 adsorbed on the surface of sintered calcium ferrite is reduced and detached by CO, releasing Fe active sites. Under low oxygen conditions, NOx is adsorbed on the surface of calcium ferrite to form a nitrate-like structure. Subsequently, the adsorbed NOx reacts with gaseous CO to generate N2 and CO2, which can simultaneously achieve the catalytic reduction of NO and NO2 and partial catalytic oxidation of CO. The catalytic efficiency gradually increases with the increase in the amount of O2 adsorbed and released on the surface of calcium ferrite. The average NOx reduction efficiency in the first 5 minutes is >40%, and the average NOx reduction efficiency in the first 10 minutes is >60%. The highest NOx reduction efficiency can reach 100%. In addition, the effect of SO2 on the CF-catalyzed CO-NOx synergistic reaction was tested, and the test results are shown in the figure below. Figure 5 The test results show that calcium ferrite has a significant absorption effect on SO2. The absorption rate of CF to SO2 can reach 100% in the first 2 minutes, and then drops to about 88%. At the same time, SO2 has a significant negative impact on NOx catalytic reduction, and the NOx conversion rate decreases by about 10% within 5 minutes.

[0041] In this embodiment, the distribution characteristics of the sintering flue gas components are as follows: the head and tail ends of the sintering machine show low CO, low NO and low sulfur characteristics due to incomplete combustion; the front and middle sections are the main sintering areas, showing high CO, high NO and low sulfur characteristics; the middle and rear sections are medium CO, medium NO and high sulfur characteristics because the sintering is nearing the end and the material layer is overly wet and the flue gas penetrates.

[0042] In this embodiment, the current sintering flue gas treatment process adopts the traditional full-bellows mixed air treatment method to purify pollutants. The amount of flue gas to be purified is large, the load of the purification equipment is high, the comprehensive utilization efficiency is low, and there is a lack of CO treatment solutions. Therefore, according to the distribution characteristics of the flue gas components of each bellows of the sintering machine, a bellows partition induced draft treatment and flue gas utilization method are designed as follows: Figure 1 shown.

[0043] In this embodiment, the front-middle section induced draft staged purification treatment method and flue gas condition control parameters are designed in combination with the sintering flue gas component distribution characteristics and the above-mentioned CO and NO catalytic effect test and condition requirements. The NOx treatment unit 5 controls the low oxygen and medium temperature conditions to treat NOx, and the CO treatment unit 7 controls the medium oxygen and high temperature conditions to treat CO and release heat. Figure 5 The CF-SO2 impact characteristics and the SO2 distribution characteristics of sintering flue gas are shown in the figure. Through the wind box partition induced draft treatment method, the high-sulfur flue gas in the middle and rear stages is dusted and desulfurized. The system can achieve a CO emission reduction of >80% and a NO emission reduction of >60% in the process. It can also reduce the flue gas treatment capacity of the desulfurization equipment by more than 40%, while reducing the processing load and energy consumption of the SCR process and reducing the comprehensive carbon emissions of the sintering process.

[0044] In this embodiment, based on the sintering process of the sintering machine, the wind box is divided into #1~#14 sub-wind boxes (not representing the actual number of wind boxes). Based on the concentration and temperature characteristics of O2, CO, NOx, and SO2 components, each sub-wind box selects #2~#6 wind boxes as the induced draft area D, and the corresponding wind box high CO, high NOx, and low sulfur flue gas is mixed into flue gas i, #7~#12 wind boxes are used as the induced draft area E, and the corresponding wind box high CO, high NOx, and high sulfur flue gas is mixed into flue gas ii, and #13~#14 wind boxes are used as the induced draft area F, and the corresponding wind box low CO, low NOx, low sulfur, and high temperature flue gas is mixed into flue gas iii. #1 wind box is used as induced draft zone C, and the corresponding wind box high oxygen gas is gas distribution i. The flue gases i~iii are used as gas distribution ii after the following treatment. The gas distribution i and part of the gas distribution ii are mixed by the gas distribution unit ⑧ and the oxygen content is adjusted to more than 18% by natural air, and then used as gas distribution iii to provide sintering gas distribution for the sintering machine. Based on the following CO and NOx reaction conditions and SO2 influence, in this embodiment, the treatment temperature of the NOx treatment unit 5 is 400-600℃, and the reaction time is greater than 600s. The treatment temperature of the CO treatment unit 7 is 600-800℃, and the reaction time is 30-60s. The design parameters of the flue gas selection of each wind box are shown in Table 1:

[0045] Table 1 Wind box partition induced draft parameter design

[0046]

[0047] Table 2 Flue gas CO and NOx treatment parameter design

[0048]

[0049] NO design treatment rate: >60%, CO design treatment rate: >80%. Combined with the following CO and NOx treatment test results and CF-SO2 influence characteristics, the design parameters of flue gas IV, flue gas V and NOx treatment unit 5, CO treatment unit 7 are shown in Table 2.

[0050] Sintering flue gas CO and NOx treatment plan: Based on the sintering hot ore temperature from high to low and the transportation direction during the ring cooling process, the ring cooling section is divided into ring cooling section I-ring cooling section V. After the flue gas II passes through the desulfurization unit and the dust removal unit, it is mixed with the flue gas I in the first gas mixing unit and enters the electrostatic precipitator unit. After mixing, it enters the NOx treatment unit as flue gas iv, and uses a gas-solid countercurrent method to sequentially contact the high-temperature sintering hot ore in the ring cooling section III and the ring cooling section II for heating and calcium ferrite catalysis. After CO-NOx synergistic NOx reduction, the flue gas iv enters the oxygen extraction and mixing unit and mixes with the flue gas III to extract oxygen. After mixing, it enters the CO treatment unit as flue gas V, and uses a gas-solid countercurrent method to oxidize CO and release heat and remove CO with the high-temperature sintering hot ore in the ring cooling section I. After CO oxidation heat release and sintering hot ore waste heat recovery, the gas is used as distribution gas II, and then enters the distribution unit according to the sintering distribution gas and oxygen content control, mixed with distribution gas I and introduced into natural air to adjust the air volume and oxygen content, and then used as distribution gas III to supply the sintering process after adjustment. The remaining distribution gas II enters the SCR deep denitrification unit, and after deep denitrification, it enters the waste heat utilization unit as purified gas for waste heat utilization, and then is discharged from the chimney in the factory.

[0051] The wind box partition air induction scheme and circulation system are shown as follows Figure 1 As shown, A is the sintering process, B is the ring cooling process, and the black arrow is the moving direction of the sintered ore.

[0052] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A flue gas circulation system for sintering CO-NOx synergistic removal and energy saving optimization, comprising a sintering module A, a wind box group and an annular cooling module B, characterized in that: It includes five smoke channels, three air distribution channels and one purified air channel, and the wind box group has an induced draft area C, an induced draft area D, an induced draft area E and an induced draft area F; The flue gas i channel is formed by the induced draft area D and the first gas mixing unit (3) and the electrostatic precipitator unit (4) being connected in one direction in sequence through pipelines. The flue gas i channel is used to transport CO-NOx treated flue gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is less than 50mg / Nm 3 , the flue gas temperature is higher than 200℃; The flue gas ii channel is formed by the induced draft area E and the desulfurization unit (1), the dust removal unit (2), and the first gas mixing unit (3) being connected in one direction in sequence through pipelines. The flue gas ii channel is used to transport high-sulfur CO-NOx treated flue gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is higher than 50mg / Nm 3 ; The flue gas iii channel is formed by the induced draft area F and the oxygen-raising gas mixing unit (6) being connected in one direction. The flue gas iii channel is used to transport oxygen-raising flue gas, specifically, the oxygen content is higher than 16%, and the SO2 concentration is higher than 50mg / Nm 3 , the flue gas temperature is higher than 500℃; The flue gas IV channel is formed by the electrostatic precipitator unit (4) sequentially connected in one direction in series with the NOx treatment unit (5) and the oxygen supply and mixing unit (6); the NOx treatment unit (5) is arranged in the ring cooling section II-ring cooling section III of the ring cooling module B; the flue gas IV channel is used to transport the NOx treated gas, specifically, the CO:O2 volume concentration ratio is greater than 2.5, and the NOx concentration is higher than 50 mg / Nm 3 , SO2 concentration is less than 50mg / Nm 3 , the flue gas temperature is higher than 150℃; The flue gas v channel is formed by the one-way connection between the oxygen supply and gas mixing unit (6) and the CO processing unit (7). The flue gas v channel is used for CO processing gas, specifically, the CO:O2 volume concentration ratio is less than 0.5, and the SO2 concentration is lower than 35 mg / Nm 3 , the flue gas temperature is higher than 500℃; The CO treatment unit (7) is respectively connected to the SCR deep denitration unit (9) and the gas distribution unit (8) to form a gas distribution channel ii and a gas distribution channel iii; The air distribution channel i is formed by the unidirectional communication between the air induction area C and the air distribution unit (8), and is used to transport high-oxygen distribution air, specifically, an oxygen content higher than 16%; The SCR deep denitration unit (9), the waste heat utilization unit (10), and the chimney are connected in series and one-way to form a purified gas channel.

2. The flue gas circulation system for sintering CO-NOx synergistic removal and energy saving optimization according to claim 1 is characterized by: The oxygen content of the distribution gas iii after being processed by the distribution unit (8) is greater than 18%.

3. The flue gas circulation system for sintering CO-NOx synergistic removal and energy saving optimization according to claim 1 is characterized by: The NOx treatment unit (5) adopts a gas-solid countercurrent passage, the treatment temperature is 400-600° C., and the reaction time is greater than 600 s.

4. The flue gas circulation system for sintering CO-NOx synergistic removal and energy saving optimization according to claim 1 is characterized by: The CO treatment unit (7) adopts a gas-solid countercurrent path, the treatment temperature is 600-800° C., and the reaction time is 30-60 seconds.

5. The method for using the flue gas circulation system for sintering CO-NOx synergistic removal and energy saving optimization according to any one of claims 1 to 4, characterized in that: include: A: Based on the temperature of the sintered hot ore from high to low and the transportation direction during the ring cooling process, the ring cooling section is divided into the ring cooling section I to the ring cooling section V. After the flue gas II passes through the desulfurization unit (1) and the dust removal unit (2), it is mixed with the flue gas I in the first gas mixing unit (3) and enters the electrostatic precipitator unit (4). After mixing, it enters the NOx treatment unit (5) as flue gas IV and sequentially contacts with the high temperature sintered hot ore in the ring cooling section III and the ring cooling section II in a gas-solid countercurrent manner for heating and calcium ferrite catalysis. After CO-NOx synergistic NOx reduction, the flue gas IV enters the oxygen extraction gas mixing unit (6) and mixes with the flue gas III to extract oxygen. After mixing, it enters the CO treatment unit (7) as flue gas V and uses a gas-solid countercurrent method to oxidize CO and release heat and remove CO with the high temperature sintered hot ore in the ring cooling section I. After CO oxidation heat release and sintering hot ore waste heat recovery, the gas is used as distribution gas II, and then enters the distribution unit (8) according to the sintering distribution gas and oxygen content control, mixed with distribution gas I and introduced into natural air to adjust the air volume and oxygen content, and after adjustment, it is supplied as distribution gas III to the sintering process. The remaining distribution gas II enters the SCR deep denitration unit (9), and after deep denitration, it enters the waste heat utilization unit (10) as purified gas for waste heat utilization, and then is discharged from the chimney in the factory.