Monocrystal lithium-rich manganese-based positive electrode active material with preferred growth of crystal face as well as preparation method and application of single crystal lithium-rich manganese-based positive electrode active material

The preparation method of single crystal lithium-rich manganese-based cathode materials through preferential growth of crystal planes solves the problems of irreversible capacity loss and voltage attenuation of existing materials in high-rate fast charging applications, achieving excellent rate performance and structural stability, and is suitable for for high-performance lithium-ion batteries.

CN118867221APending Publication Date: 2024-10-29广东聚圣科技有限公司

Patent Information

Application Number
CN202410899619.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing lithium-rich manganese-based cathode materials have problems such as irreversible capacity loss, rapid capacity/voltage attenuation, and poor safety performance during the cycle process, making it difficult to adapt to the application requirements of high-rate fast charging.

Method used

The preparation method of single crystal lithium-rich manganese-based cathode active material with preferential growth of crystal planes is adopted. Through pre-reaction of polycarboxylic acid, sintering aid and water-alcohol mixed solvent, two-stage sintering is performed to optimize the physical and chemical characteristics and crystal structure of the intermediate. , forming long-range ordered elongated single crystal materials, optimizing crystal planes and crystal structures, and improving structural stability and dynamic properties.

Benefits of technology

It achieves excellent rate performance of the material, improves structural stability, thermal stability and compaction density, inhibits oxygen release and transition metal ion migration, enhances crack resistance and reversibility, and takes into account excellent capacity, rate and cycle voltage stability. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867221A_ABST
    Figure CN118867221A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of battery materials, and particularly relates to a single crystal lithium-rich manganese-based positive electrode active material with preferred growth of a crystal face, which is a long-strip-shaped single crystal lithium-rich manganese-based positive electrode active material with 001, 100 dominant crystal faces. The invention also provides a preparation method of the material, which specifically comprises the following steps: pre-reacting precursor raw materials containing a manganese source and an M source in polycarboxylic acid, a sintering aid and an alcohol-water mixed solvent, and then drying to obtain an intermediate; and carrying out two-stage sintering on the intermediate to obtain the product. The invention also provides an application of the material in a lithium ion battery. The material provided by the invention has excellent crystal face and crystal result, and has excellent fast charge and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium-ion battery materials, and more specifically to the field of cathode materials for lithium-ion batteries. Background Art

[0002] Currently, the demands in fields such as portable electronic devices, electric vehicles, and energy storage power grids have promoted the development and utilization of high-performance lithium-ion batteries. As the core of the four major components of lithium-ion batteries, the cathode material plays a decisive role in the cost and performance of lithium-ion batteries. In particular, in recent years, the lithium-rich manganese-based cathode material has attracted much attention due to its extremely high specific capacity and low raw material cost. However, during its service process, there are generally problems such as serious irreversible capacity loss, rapid capacity / voltage decay, and poor safety performance, which restrict the large-scale application of high-performance lithium-ion batteries. The above problems are mainly caused by irreversible oxygen release, phase structure transformation, interfacial side reactions, and intergranular / intracrystalline crack growth at the surface and interface of the lithium-rich manganese-based cathode material with low specific surface area and low thermal stability during the cycling process. So far, modification methods such as element doping, surface coating, and chemical treatment have to some extent compensated for the deficiencies of the lithium-rich manganese-based cathode material, but there is still much room for improvement. Single crystal engineering can fundamentally solve the inherent problems related to the structure and interface of the cathode material, supplemented by strategies such as element doping and composition optimization, effectively improving the comprehensive properties such as the structural stability, thermal stability, and kinetic properties of the cathode material.

[0003] Some single crystal lithium-rich manganese-based materials are also disclosed in the prior art. For example, the Chinese patent document with the publication number CN117712363A discloses a submicron single crystal lithium-rich manganese-based cathode material with the chemical formula xLi2MnO3·(1-x)LiTMO2, where: 0 < x < 1, and TM is a soluble transition metal. Another example is that the Chinese patent document with the publication number CN117317210A discloses a quasi-single crystal lithium-rich manganese-based cathode material and its preparation method and application. The quasi-single crystal lithium-rich manganese-based cathode material comprises quasi-single crystal particles formed by primary particles with an average particle size of 400 nm to 700 nm, and the quasi-single crystal particles satisfy the following relationships: 5 ≤ K < 15; 0.8 m2 / g ≤ α ≤ 2.0 m2 / g, 1.5 μm ≤ D50 < 4.0 μm, 0.4 μm ≤ Dmin < 0.8 μm, where α is the specific surface area of the quasi-single crystal particles, D50 is the median particle size of the quasi-single crystal particles, Dmin is the minimum particle size of the quasi-single crystal particles, and K is the number of primary particles included in the quasi-single crystal particles.

[0004] Although some optimization schemes for single crystals are disclosed in the prior art, the existing methods are still difficult to effectively control the crystal structure and grain size of single crystals, making it still difficult to adapt to the application requirements of high-rate fast charging. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a single-crystal lithium-rich manganese-based positive electrode active material with preferential growth on the crystal plane, aiming to provide a material with excellent rate performance.

[0006] The second object of the present invention is to provide a method for preparing the single crystal lithium-rich manganese-based positive electrode active material with preferential growth of the crystal face, aiming to prepare a new material with the crystal face characteristics.

[0007] The third object of the present invention is to provide a single crystal lithium-rich manganese-based positive electrode active material with preferential growth on a crystal face for use in lithium-ion batteries.

[0008] The fourth object of the present invention is to provide a lithium-ion battery and a positive electrode and positive electrode material thereof comprising the single-crystal lithium-rich manganese-based positive electrode active material with preferential growth on the crystal plane.

[0009] A single crystal lithium-rich manganese-based positive electrode active material with preferential growth of crystal faces is a single crystal lithium-rich manganese-based positive electrode active material with 001 and 100 dominant crystal faces and a long strip shape.

[0010] The present invention studies show that the single-crystal lithium-rich manganese-based material with the advantageous crystal plane and morphology can exhibit excellent electrochemical properties such as rate capability.

[0011] The chemical formula of the single crystal lithium-rich manganese-based positive electrode active material is Li a Mn b M c O2, wherein M comprises Ni and / or Co; wherein 1 <a≤1.5;0.4≤b≤0.8;0≤c<0.4;

[0012] Preferably, the a is 1.1 to 1.3; the molar ratio of b / c is 1 to 3:1, and b+c is equal to 0.7 to 0.9.

[0013] In the present invention, the a can be 1.2. The molar ratio of b / c is 2 to 2.5:1. b+c is equal to 0.8.

[0014] The present invention also provides a method for preparing a single crystal lithium-rich manganese-based positive electrode active material with preferential growth of crystal faces, wherein a precursor raw material containing a manganese source and an M source is pre-reacted in a polycarboxylic acid, a sintering aid, and an alcohol-water mixed solvent, and then dried to obtain an intermediate; and then the intermediate is sintered in two stages to obtain;

[0015] The sintering aid is a component that can be liquefied during the sintering stage, and includes component A and component B, wherein component A is at least one of LiCl, LiOH, LiF, LiNO3, Li2CO3, LiAc, and Li2O; and component B is at least one heterogeneous salt including NaCl, KCl, KNO3, NaNO3, K2B4O7, and Na2B4O7;

[0016] The Li content of component A in the sintering aid is 1.48 to 1.55 times the total molar amount of Mn+M in the precursor raw material; the weight ratio of component A to component B is 1:(0.005 to 0.03).

[0017] The present invention innovatively pre-reacts the precursor raw materials in the sintering aid containing component A and component B and a water-alcohol mixed solvent, which can optimize the physicochemical characteristics of the intermediate, and further perform a subsequent two-stage sintering treatment, which can facilitate the localized liquefaction sintering of the in-situ composite sintering aid in the intermediate, so as to synergistically optimize the crystal, crystal structure and exposure site of the single crystal. The surface morphology of the lithium-rich manganese-based positive electrode material obtained by the method of the present invention is smooth and regular, the bulk structure is long-range ordered, and it is in the form of long strips, with the crystal face facing <001> and <100> The crystal orientation-preferential growth is beneficial to improve the electrode reaction kinetics and the uneven Li + Concentration gradient distribution. Secondly, the single crystal particles with high mechanical strength have good crack resistance, which is sufficient to withstand higher stress and alleviate lattice distortion during the cycle process, effectively improving structural stability, thermal stability and compaction density. Moreover, the material can also inhibit oxygen release and transition metal ion migration, improving structural stability and reversibility.

[0018] In the present invention, the combined in-situ participation of component A and component B in the pre-reaction and the joint control of the ratio parameters of the reaction solvent and the sintering aid are the key to synergistically optimizing the intermediate structure, facilitating localized liquefaction sintering, improving the grain size, crystal structure and crystal surface exposure of the prepared material, and thus improving the fast charging and other properties of the material.

[0019] In the present invention, the manganese source comprises a water-soluble salt of Mn(II), and may further be at least one of nitrate, sulfate, acetate, and chloride;

[0020] In the present invention, the M source is a water-soluble salt of the M metal, and may further be at least one of nitrate, sulfate, acetate, and chloride;

[0021] In the present invention, in the precursor material, the Mn / (Mn+M) is 70-80 mol%.

[0022] In the present invention, the polycarboxylic acid is a dibasic to tetrabasic carboxylic acid having a carbonic acid content of 6 or less, and is preferably at least one of oxalic acid and citric acid.

[0023] In the present invention, the combination of the polycarboxylic acid and the alcohol-water system can regulate the dispersion of Mn and M, so as to induce the preferential growth of the dominant crystal plane described in the present invention.

[0024] In the present invention, the weight ratio of the polycarboxylic acid to the manganese source is 2 to 10 times, and further 3 to 7 times.

[0025] In the present invention, in the sintering aid, the component A comprises at least one of LiCl, LiOH, LiNO3, Li2CO3, and LiAc;

[0026] Preferably, the component B includes at least one of NaCl, NaNO3, and Na2B4O7. Studies have shown that the use of the preferred component B, especially Na2B4O7 as component B, can be further combined with other processes to further induce the material's dominant crystal plane and grain structure, which helps to further improve the fast charging and stability of the prepared material.

[0027] Preferably, the weight ratio of component A to component B is 1:(0.01-0.03), and more preferably 1:0.01-0.02. Studies have shown that under a favorable ratio, the advantageous crystal plane and grain structure of the material can be further induced, which helps to further improve the fast charging and stability of the prepared material.

[0028] In the present invention, in the alcohol-water mixed solvent, the alcohol includes C1-C4 alcohol, further at least one of ethanol and ethylene glycol. Further, it is a mixed alcohol of ethanol and ethylene glycol in a volume ratio of 1 to 3:1. The study unexpectedly showed that under the mixed alcohol, combined with the process and parameters, the dominant crystal plane of the material can be further optimized, the grain and crystal structure can be improved, and the fast charging and high rate stability of the prepared material can be further enhanced.

[0029] Preferably, in the alcohol-water mixed solvent, the volume content of alcohol is 20 to 70 v%, and can further be 50 to 65 v%;

[0030] Preferably, the temperature of the pre-reaction is 60 to 90°C;

[0031] Preferably, the pre-reaction time is 1 to 5 hours.

[0032] Preferably, after the pre-reaction, the intermediate can be obtained by freeze drying or vacuum drying.

[0033] In the present invention, the two-stage sintering process is carried out in an oxygen-containing atmosphere;

[0034] Preferably, the temperature of the first sintering and heat preservation process and the second sintering and heat preservation process of the two-stage sintering process is 200-900°C, preferably 400-600°C, and more preferably 500-600°C; the temperature of the second sintering and heat preservation process is 700-900°C, preferably 800-900°C;

[0035] The first stage sintering and heat preservation time is 3 hours or more, preferably 4 to 12 hours; the second stage sintering and heat preservation time is 10 hours or more, preferably 15 to 20 hours.

[0036] The present invention also provides a single crystal lithium-rich manganese-based positive electrode active material prepared by the preparation method with preferential growth of crystal faces, which has <001> and <100> The characteristics of preferential growth in crystal direction are long strips in shape.

[0037] Moreover, the material with the characteristics obtained by the preparation method can unexpectedly take into account excellent fast charging, long cycle and other effects.

[0038] The present invention also provides an application of a single crystal lithium-rich manganese-based positive electrode active material with preferential crystal face growth obtained by the preparation method, which is used as a positive electrode active material for preparing a lithium-ion battery.

[0039] The present invention also provides a positive electrode of a lithium ion battery, which comprises a single crystal lithium-rich manganese-based positive electrode active material with preferential growth on a crystal face obtained by the preparation method.

[0040] The present invention also provides a lithium ion battery, which comprises the positive electrode of the present invention.

[0041] In the present invention, the materials of the present invention can be used to prepare the required lithium-ion battery and its positive electrode and positive electrode material based on the conventional principles and means in lithium-ion batteries.

[0042] Beneficial Effects

[0043] The present invention uses the low-melting-point component A and component B in a synergistic combination as a sintering aid, and uses them to participate in the in-situ pre-reaction of the precursor raw material in situ, and further controls the process parameters such as the sintering aid and the pre-reaction solvent, so that the grain growth and the preferential epitaxial growth of the grains can be induced to grow into long strip-shaped grains, so that synergy can be achieved, the structure of the intermediate can be optimized, and a localized liquid phase reaction microcavity can be constructed in the sintering stage, and the crystal structure, grains and crystal planes of the material can be optimized. In addition, a stable chemical bond can be formed with TM at the octahedral / tetrahedral site of the positive electrode material lattice, thereby inhibiting the lattice oxygen -The irreversible release of TM and the migration of TM from the octahedral site to the Li site reduce the layered / spinel / rock salt structural phase transition; it can also play the role of interlayer pillar and pinning effect, alleviate the lattice distortion during the cycle, prevent the collapse of the interlayer, and effectively stabilize the crystal structure; and in situ form the spinel phase and oxygen vacancies on the surface layer, effectively capture the active oxygen escaping from the bulk phase, synergistically regulate the oxygen redox behavior, thereby inhibiting oxygen release, TM dissolution and interface side reactions, and improving the structural stability and reversibility.

[0044] The positive electrode material obtained by the method of the present invention is a micron-sized single crystal with smooth surface morphology and long-range ordered bulk phase, and the internal lattice is continuous and consistent without grain boundaries, which can not only improve electronic conductivity and ion conductivity, improve electrode reaction kinetics, but also alleviate Li + The concentration gradient distribution and anisotropic stress-strain inhibit crack growth and prevent electrolyte penetration and corrosion along the new surface. In addition, the single crystal particles with high mechanical strength have good crack resistance, which is sufficient to withstand higher stress, and improve structural stability, thermal stability and compaction density. The research of the present invention shows that the material can take into account excellent capacity, rate, cycle and voltage stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the SEM image of Example 1 (schematic diagram of micron-scale particle size);

[0046] Figure 2 TEM image (single crystal structure schematic diagram) of Example 1;

[0047] Figure 3 EBSD diagram of Example 1 (schematic diagram of preferred crystal orientation);

[0048] Figure 4 It is a comparison diagram of the rate performance of Example 1 and Comparative Example 1;

[0049] Figure 5 1 is a comparison chart of the cycle performance between Example 1 and Comparative Example 1; DETAILED DESCRIPTION

[0050] Example 1

[0051] Step 1:

[0052] 3.81521g of manganese nitrate aqueous solution (Mn(NO3)2, 50wt%), nickel nitrate hexahydrate ((Mn / Ni molar ratio is 0.666:0.284)) and a sintering aid (component A is lithium nitrate, component B is Na2B4O7, wherein Li / (Mn+Ni) in component A is 1.52, and the weight ratio of component A to component B is 1:0.01) are dissolved in ethanol to form a mixed solution (the water / ethanol volume ratio in the system is 2:3), and then 10.0856g of polyacid (oxalic acid, H2C2O4) in ethanol solution is dripped into the above mixed solution, and a pre-reaction is carried out at 80°C for 2-3h, and then the solvent is evaporated to obtain an intermediate;

[0053] Step 2:

[0054] The intermediate of step 1 is sintered in air, and the sintering mechanism is: heating from room temperature to 500°C at a rate of 2°C / min and keeping the temperature for 5h, then heating to 900°C at a rate of 1°C / min and keeping the temperature for 1200min, and then cooling to room temperature with the furnace to obtain the modified material.

[0055] The XRD of the cathode material prepared by the above method shows that the main diffraction peak of the obtained material is the α-NaFeO2 structure of the hexagonal R-3m space group, and it also has a weak diffraction peak of 20-25° related to the monoclinic C2 / m space group. It is a typical lithium-rich material with a lower degree of Li / Ni mixing and a more ordered layered structure. The SEM and TEM analysis results are shown in Figure 1 , 2 As shown in the figure, the modified material is a long-range ordered single crystal material at the micrometer scale, which is successfully calibrated as a layered structure of the R-3m space group. Figure 3 As shown, the EBSD image is mainly composed of polygonal blocks with red and green tones. The color inside a single block is uniform and the external boundary is clear and complete, indicating that most of the grains of the modified material have roughly similar orientations, mainly

[001] and

[100] .

[0056] test:

[0057] The modified positive electrode material prepared by the above method, acetylene black and PVDF were mixed uniformly in a mass ratio of 8:1:1 to form a slurry, which was uniformly coated on an aluminum foil, cut into a positive electrode sheet with a diameter of 12 mm, and a lithium metal sheet was used as a negative electrode, Celgard 2500 was used as a separator, and a 1.2M LiPF6 EC / EMC / DMC (volume ratio 1:2:2) solution was used as an electrolyte. A CR2016 type button battery was assembled in an argon-filled glove box, which is the battery of Example 1. The above battery was subjected to a charge and discharge cycle test, wherein the test voltage range was 2 to 4.8 V and the test temperature was 30°C.

[0058] Comparative Example 1

[0059] 2 g of lithium-rich material precursor A (Mn-Ni carbonate precursor, wherein the molar ratio of Mn to Ni is the same as in Example 1) and lithium carbonate (Li2CO3; the amount of lithium element is the same as in Example 1) are solid-phase mixed evenly, sintered in air, heated from room temperature to 500°C at a rate of 2°C / min and kept warm for 5 h, then heated to 900°C at a rate of 1°C / min and kept warm for 1200 min, and then cooled to room temperature in the furnace to obtain a lithium-rich material.

[0060] like Figure 4 The figure shows the rate performance test. The discharge capacity of the battery in comparative example 1 at a current density of 10C is only 104 mAh / g, while the discharge capacity of the battery in embodiment 1 is as high as 161 mAh / g, and the rate performance is significantly improved.

[0061] The comparison results of cycle performance are as follows Figure 5 As shown, the initial discharge capacity of Example 1 at 1C is 210 mAh / g, and after 200 cycles, the capacity retention rate is 86%, while the initial discharge capacity of the battery of Comparative Example 1 is 200 mAh / g, and the 200 cycle stability is 71%.

[0062] Example 2

[0063] Compared with Example 1, the only difference is that the amount of component B in the sintering aid is changed. The experimental groups are:

[0064] Group A: The weight ratio of component A to component B is 1:0.02;

[0065] Group B: The weight ratio of component A to component B is 1:0.005;

[0066] Group C: Compared with Group A, the difference is that component A is lithium carbonate and lithium nitrate with a weight ratio of 0.1:1, and the total molar amount of Li remains unchanged;

[0067] Tested according to the method of Example 1, the results are:

[0068] Group A: The battery of the material of this embodiment has a 10C rate performance of 154 mAh / g, a 1C capacity of 207 mAh / g, and a capacity retention rate of 84% after 200 cycles.

[0069] Group B: The battery of the material of this embodiment has a 10C rate performance of 143 mAh / g, a 1C capacity of 208 mAh / g, and a capacity retention rate of 75% after 200 cycles.

[0070] Group C: The battery of the material of this embodiment has a 10C rate performance of 151 mAh / g, a 1C capacity of 204 mAh / g, and a capacity retention rate of 82% after 200 cycles.

[0071] Example 3

[0072] Compared with Example 1, the only difference is that NaNO3 is selected as the sintering aid B, and the other steps remain unchanged. The battery of the example material has a 10C rate performance of 152 mAh / g, a 1C capacity of 206 mAh / g, and a capacity retention rate of 82% after 200 cycles.

[0073] Example 4

[0074] Compared with Example 1, the only difference is that KCl is selected as the sintering aid B, and the other steps remain unchanged. The battery of the example material has a 10C rate performance of 147 mAh / g, a 1C capacity of 204 mAh / g, and a capacity retention rate of 81% after 200 cycles.

[0075] Example 5

[0076] Compared with Example 1, the only difference is that in step 2, the first stage sintering temperature is 600°C, the holding time at the first stage sintering temperature is 10 hours, the second stage sintering temperature is 850°C, and the sintering time is 900 minutes. Other operations and parameters are the same as in Example 1.

[0077] The test results were as follows: the battery material of this embodiment had a 10C rate performance of 148 mAh / g, a 1C capacity of 204 mAh / g, and a capacity retention rate of 80% after 200 cycles.

[0078] Example 6

[0079] Compared with Example 1, the only difference is that the added polyacid is citric acid, which is 6 times the weight of the manganese source, and the other operations and tests are the same as Example 1. The results are: the battery assembled with the material has a 10C rate performance of 158 mAh / g, a 1C capacity of 209 mAh / g, and a capacity retention rate of 85% after 200 cycles.

[0080] Example 7

[0081] Compared with Example 1, the only difference is that the type of alcohol in the solvent is changed, specifically:

[0082] Group A: the alcohol is ethylene glycol, which has the same volume as the ethanol in Example 1;

[0083] Group B: alcohol is a mixed alcohol of ethanol and ethylene glycol in a volume ratio of 2:1, and the total volume of the mixed alcohol is the same as the ethanol in Example 1;

[0084] The test was carried out according to the method of Example 1, and the results were:

[0085] Group A: 10C rate performance is 159mAh / g, 1C capacity is 208mAh / g, and capacity retention is 84% ​​after 200 cycles.

[0086] Group B: 10C rate performance is 165mAh / g, 1C capacity is 210mAh / g, and capacity retention is 89% after 200 cycles.

[0087] It can be seen from Examples 1 and 7 that the use of the special mixed alcohol-water system can further synergistically improve the crystal plane, grains and crystal structure of the material, and unexpectedly further enhance the fast charging and high-rate stability of the material.

[0088] Comparative Example 2

[0089] Compared with Example 1, the only difference is that no pre-reaction assisted by a sintering aid is performed, but the lithium-rich material precursor A is directly mixed with the sintering aid to directly perform the treatment in step 2. Other operations and parameters are the same as those in Example 1. The 10C rate performance is 98 mAh / g, the 1C capacity is 197 mAh / g, and the capacity retention rate after 200 cycles is 72%.

[0090] Comparative Example 3

[0091] Compared with Example 1, the only difference is that the pre-reaction assisted by the sintering aid is not performed, that is, in step 1, the sintering aid is not added in the pre-reaction stage, and the product is obtained by drying after the pre-reaction, and the product and the sintering aid are mixed and used as an intermediate to perform the treatment in step 2. The 10C rate performance is 112 mAh / g, the 1C capacity is 201 mAh / g, and the capacity retention rate after 200 cycles is 75%.

[0092] Comparative Example 4

[0093] Compared with Example 1, the only difference is that the equal volume of ethanol used in step 1 is replaced by water, and the other operations and parameters are the same as Example 1. The 10C rate performance is 105 mAh / g, the 1C capacity is 199 mAh / g, and the capacity retention rate after 200 cycles is 73%.

[0094] Comparative Example 5

[0095] Compared with Example 1, the only difference is that in step 1, component B is not added to the sintering aid, and other operations and parameters are the same as Example 1. The 10C rate performance is 115 mAh / g, the 1C capacity is 201 mAh / g, and the capacity retention rate after 200 cycles is 72%.

Claims

1. A single-crystal lithium-rich manganese-based positive electrode active material with preferential growth on crystal faces, It is characterized in that It is a single-crystal lithium-rich manganese-based positive electrode active material with 001 and 100 dominant crystal planes and a long strip-shaped morphology; Preferably, the chemical formula of the single crystal lithium-rich manganese-based positive electrode active material is Li a Mn b M c O 2 , wherein M comprises Ni and / or Co; wherein 1 <a≤1.5;0.4≤b≤0.8;0≤c<0.4; Preferably, the a is 1.1 to 1.3; the molar ratio of b / c is 1 to 3:1, and b+c is equal to 0.7 to 0.

9.

2. A method for preparing a single-crystal lithium-rich manganese-based positive electrode active material with preferential growth of crystal faces, It is characterized in that Preliminary reaction of precursor materials including manganese source and M source in polycarboxylic acid, sintering aid and alcohol-water mixed solvent is performed, followed by drying to obtain an intermediate; and the intermediate is sintered in two stages to obtain; The sintering aid is a component that can be liquefied during the sintering stage, and includes component A and component B, wherein component A is LiCl, LiOH, LiF, LiNO 3 , Li 2 CO 3 、LiAc、Li 2 O; the component B comprises NaCl, KCl, KNO 3 、NaNO 3 , K 2 B 4 O 7 、Na 2 B 4 O 7 at least one heterogeneous salt of; The Li content of component A in the sintering aid is 1.48 to 1.55 times the total molar amount of Mn+M in the precursor raw material; the weight ratio of component A to component B is 1:(0.005 to 0.05).

3. The preparation method according to claim 2, It is characterized in that The manganese source comprises a water-soluble salt of Mn(II), preferably at least one of nitrate, sulfate, acetate, and chloride; Preferably, the M source is a water-soluble salt of M metal.

4. The preparation method according to claim 2, It is characterized in that The polycarboxylic acid is a dibasic to tetrabasic carboxylic acid having a carbonic acid content of 6 or less; preferably at least one of oxalic acid and citric acid; Preferably, the weight ratio of the polycarboxylic acid to the manganese source is 2 to 10 times, further 3 to 7 times.

5. The preparation method according to claim 2, It is characterized in that The sintering aid, the component A includes LiCl, LiOH, LiNO 3 , Li 2 CO 3 , LiAc; Preferably, the component B includes NaCl, NaNO 3 、Na 2 B 4 O 7 At least one of; Preferably, the weight ratio of component A to component B is 1:(0.01-0.03).

6. The preparation method according to claim 2, It is characterized in that In the alcohol-water mixed solvent, the alcohol includes C1 to C4 alcohol; Preferably, the volume content of alcohol in the alcohol-water mixed solvent is 20 to 70 v%; Preferably, the temperature of the pre-reaction is 60 to 90°C; Preferably, the pre-reaction time is 1 to 5 hours; Preferably, after the preliminary reaction, the intermediate can be obtained by freeze drying or vacuum drying.

7. The preparation method according to claim 2, It is characterized in that The two-stage sintering process is carried out in an oxygen-containing atmosphere; Preferably, the temperature of the first sintering and heat preservation process and the second sintering and heat preservation process of the two-stage sintering process is 200-900°C, preferably 400-600°C, and more preferably 500-600°C; the temperature of the second sintering and heat preservation process is 700-900°C, preferably 800-900°C; The first stage sintering and heat preservation time is 3 hours or more, preferably 4 to 12 hours; the second stage sintering and heat preservation time is 10 hours or more, preferably 15 to 20 hours.

8. Use of a single crystal lithium-rich manganese-based positive electrode active material with preferential growth on a crystal face according to claim 1 or a single crystal lithium-rich manganese-based positive electrode active material with preferential growth on a crystal face obtained by the preparation method according to any one of claims 2 to 7, It is characterized in that It is used as positive electrode active material to prepare lithium-ion batteries.

9. A positive electrode of a lithium-ion battery, It is characterized in that The invention comprises the single crystal lithium-rich manganese-based positive electrode active material with preferential growth on the crystal face as described in claim 1 or the single crystal lithium-rich manganese-based positive electrode active material with preferential growth on the crystal face obtained by the preparation method according to any one of claims 2 to 7.

10. A lithium ion battery, It is characterized in that The positive electrode according to claim 9 is included.

Citation Information

Patent Citations

  • Monocrystal-like lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

    CN117317210A

  • Submicron single crystal lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

    CN117712363A

Cited By

  • Positive electrode active material and preparation method and application thereof

    CN120048888A

  • A positive electrode active material, its preparation method and application

    CN120048888B

  • Method for preparing single-crystal-state lithium-rich manganese-based positive electrode material by molten salt method, positive electrode material prepared by method, positive electrode and battery

    CN120914242A