High-toughness MoNbTaW refractory alloy and preparation method thereof
By introducing La2O3 particles into MoNbTaW alloys to generate composite oxides, high-energy ball milling and discharge plasma sintering technology, the dendrites and components segregation problems in difficult-to-fusion alloys are solved, significantly improving the strength and toughening properties of the alloys, and suitable for a wide range of Application environment.
Patent Information
- Application Number
- CN202410951266.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
AI Technical Summary
The existing technology for preparing refractory alloys cannot effectively solve the problem of segregation of coarse dendrites and chemical compositions, resulting in low toughness of MoNbTaW alloys and the inability to introduce a second phase into refractory alloys for strengthening, limiting its application environment.
By introducing La2O3 particles into the MoNbTaW alloy, two composite oxides, La0.33TaO3 and La4.8Ta22O62, are generated as the second phase. Through high-energy ball milling and discharge plasma sintering technology, the particle size and distribution are controlled to improve the toughening performance of the alloy. and reduce brittleness.
It significantly improves the comprehensive mechanical properties of MoNbTaW alloy, including room temperature compression yield strength and fracture strain, improves its stability and toughness at high temperatures, and is suitable for a wider range of application environments.
Smart Images

Figure CN118880149A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-strength and toughness refractory alloy and a preparation method thereof, and belongs to the technical field of refractory alloy material preparation. Background Art
[0002] High entropy alloys have good mechanical stability, oxidation resistance, wear resistance, corrosion resistance and high-temperature thermal stability, and have great development potential. In recent years, high entropy alloys composed of refractory metals have the advantages of both refractory alloys and high entropy alloys, especially high hardness, high toughness and good stability at high temperatures. The MoNbTaW high entropy alloy prepared by Senkov et al. has good thermal stability, its phase structure does not change after long-term annealing at high temperature, and its comprehensive mechanical properties are excellent.
[0003] From the development of refractory alloys, it can be found that vacuum arc melting is currently the most common method for preparing refractory alloy bulk materials, but this technology cannot solve the problems of coarse dendrites and chemical composition segregation, which makes the toughness of MoNbTaW alloy relatively low and the service environment limited. In addition, vacuum arc melting cannot actively introduce a second phase into the refractory alloy for strengthening, so the spark plasma sintering method is used to prepare MoNbTaW refractory alloy, and La2O3 particles are introduced into it to form La2O3 composite with the matrix. 0.33 TaO3 and La 4.8 Ta 22 O 62 The two composite oxides act as the second phase to strengthen the alloy matrix, improving strength and toughness while reducing brittleness. Summary of the invention
[0004] In view of the problem that the comprehensive mechanical properties of refractory alloys in the prior art are not ideal, the first object of the present invention is to provide a high-strength and tough refractory alloy with excellent comprehensive mechanical properties.
[0005] The second object of the present invention is to provide a method for preparing a high-strength and tough refractory alloy. By doping a transition metal refractory alloy with rare earth oxides, the prepared refractory alloy has reduced brittleness and significantly improved toughness, thereby obtaining a high-strength and tough refractory alloy with excellent comprehensive mechanical properties. The preparation method provided by the present invention is simple and easy to operate.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The invention discloses a high-strength and tough refractory alloy, wherein the refractory alloy comprises a refractory alloy matrix and La dispersed in the refractory alloy matrix. 0.33 TaO3 and La 4.8 Ta 22 O 62 Two kinds of composite oxide particles; La0.33 TaO3 and La 4.8 Ta 22 O 62 The sizes of the two composite oxide particles are both less than 600 nm, preferably less than or equal to 500 nm, and more preferably 50 to 500 nm; they are dispersed at the grain boundaries; La 0.33 TaO3 and La 4.8 Ta 22 O 62 The total molar amount of the two composite oxide particles accounts for 0.1-1 at%, preferably 0.4-0.6 at% of the refractory alloy. The refractory alloy matrix is composed of transition metal elements, and the transition metal elements are composed of four elements: Nb, Mo, W, and Ta.
[0008] The inventors found that the addition of La2O3 particles during the preparation process would combine with Ta and O in the matrix to generate La 0.33 TaO3 and La 4.8 Ta 22 O 62 The two composite oxides not only act as second phase particles to strengthen the alloy and improve its strength, but also absorb oxygen at the grain boundaries and within the grains to reduce the brittleness of the alloy, thereby obtaining a high-strength and tough refractory alloy.
[0009] As a preferred solution, the atomic percentage of any transition metal element in the refractory alloy matrix is 24.5-25.5 at.%.
[0010] The invention discloses a method for preparing a high-strength and tough refractory alloy. The method comprises the following steps: preparing transition metal element powder and La2O3 powder according to a designed ratio, high-energy ball milling to obtain a mixed powder, and then subjecting the refractory alloy mixed powder after high-energy ball milling to discharge plasma sintering to obtain a high-strength and tough refractory alloy material. The average particle size of the transition metal element powder is less than or equal to 10 μm, and the average particle size of La2O3 is less than or equal to 2 μm.
[0011] In the preparation method of the refractory alloy of the present invention, La2O3 is used to react with the MoNbTaW alloy matrix to purify the grain boundary and strengthen the second phase, which greatly reduces the brittleness of the MoNbTaW alloy after oxygen absorption and improves the mechanical properties of the refractory alloy.
[0012] The inventors found that the ball milling parameters directly affect the final sample structure. If the ball milling time is too short, the degree of alloying will be insufficient, and partial precipitated phases will be easily formed. In addition, La2O3 will not be finely dispersed at the matrix grain boundaries, and will easily aggregate in larger particles. If the ball milling time is too long, oxidation will occur, which will lead to a decrease in the mechanical properties of the alloy.
[0013] In a preferred embodiment, the mass fraction of La2O3 in the mixed powder is 0.2-1.5%, preferably 0.4-0.6%. In the present invention, when La2O3 exceeds 0.6wt%, if the addition amount is 1% or 1.5% (compared with the solution of introducing 0.45-0.55%), the fracture toughness of the product will be significantly reduced.
[0014] In a preferred embodiment, the average particle size of the transition metal element powder is 0.5-10 μm, and the average particle size of La2O3 is 0.1-2 μm.
[0015] In a preferred embodiment, the parameters of the high-energy ball milling are: a ball-to-material mass ratio of 9 to 11:1, a ball milling speed of 200 to 400 rpm, preferably 250 to 350 rpm, and a ball milling time of 20 to 50 hours, preferably 28 to 42 hours. In the present invention, when the ball milling time is too long, such as 50 hours and the speed is greater than or equal to 350 rpm, the yield strength and fracture strain of the product during room temperature compression will both decrease significantly.
[0016] Further preferably, the high energy ball milling is dry ball milling.
[0017] The inventors found that the uniform mixing and crushing degree of the powder during the ball milling process will affect the microscopic composition and performance of the subsequent samples. Too low a speed and too short a time of ball milling will lead to insufficient uniformity of powder crushing and mixing, resulting in segregation and the inability of La2O3 to be fine and dispersed. Too high a speed and too long a time of ball milling will lead to excessive activity of the refined particles, and it is easy to cause caking, cold welding, and uneven distribution of La2O3 secondary agglomeration during the ball milling process, affecting the material properties.
[0018] In a preferred solution, the refractory alloy powder is first crushed by alternating forward and reverse ball milling in an argon atmosphere to obtain a uniformly mixed fine powder, and then subjected to spark plasma sintering to obtain a high-strength and tough refractory alloy.
[0019] Further preferably, the forward and reverse alternating ball milling is carried out in a cycle of forward rotation-stop-reverse rotation-stop, and the time for any one of the forward rotation, stop, reverse rotation and stop is 20 to 30 minutes.
[0020] The inventors found that the fine powder obtained by crushing the refractory alloy powder by alternating forward and reverse ball milling has uniform particle size, good crushing effect and excellent product performance, and finally a high-strength and tough refractory alloy is obtained by spark plasma sintering. If the above-mentioned ball milling method is not adopted, the performance of the final product will be weakened to a certain extent (compared with the cycle of forward rotation-stop-reverse rotation-stop, the time for any forward rotation, stop, reverse rotation and stop is 20 to 30 minutes and the rotation speed is 250 to 400 rpm).
[0021] In a preferred embodiment, the spark plasma sintering is carried out under vacuum conditions. The process of spark plasma sintering is: heating to 1600-2100°C, more preferably 1800-2000°C, at a heating rate of 80-120°C / min, keeping the temperature for 8-15 minutes, and cooling to room temperature. The pressure of the spark plasma sintering is 30-50 MPa.
[0022] The inventors have found that by using spark plasma sintering and controlling the conditions within the above-mentioned range, a refractory alloy with fine grains, high density and excellent performance can be obtained. However, if the sintering temperature is too low, the material cannot be densified; if it is too high, the grains grow, resulting in a decrease in performance; and if the pressure is too low, the material density is insufficient and the material performance is decreased.
[0023] As a further preference, the ball-to-material mass ratio is preferably 10:1; the ball milling speed is 350 rpm; the ball milling is carried out in a cycle of forward rotation-stop-reverse rotation-stop, each step is carried out in a cycle of 30 minutes (i.e., forward rotation for 30 minutes, stop for 30 minutes, then reverse rotation for 30 minutes, stop for 30 minutes, and then forward rotation for 30 minutes, and so on), and the ball milling is carried out for 40 hours to obtain a powder mixture; in terms of mass percentage, when the powder mixture contains 17.2-17.6% Mo, 16.5-17.1% Nb, 32.5-33.2% Ta, 33-33.7% W, and the balance is La2O3,
[0024] The powder mixture was made into a block by spark plasma sintering, with a sintering pressure of 40MPa, vacuum conditions, and heated to 2000℃ at a heating rate of 80℃ / min, and kept at this temperature for 10 minutes, and then cooled with the furnace to obtain a MoNbTaW-La2O3 refractory alloy block. The room temperature compressive yield strength of the obtained MoNbTaW-La2O3 refractory alloy block was 1750MPa, and the fracture strain was 30%.
[0025] Principles and advantages
[0026] The present invention provides a high-strength and tough refractory alloy, wherein the refractory alloy comprises a refractory alloy matrix and La dispersed in the refractory alloy matrix. 0.33 TaO3 and La 4.8 Ta 22 O 62 The present invention improves the mechanical properties of the refractory alloy through the second phase strengthening mechanism to obtain a high-strength and tough refractory alloy.
[0027] The preparation method of the present invention first prepares uniform mixed refractory alloy powder by high-energy ball milling, and obtains loose powder to facilitate subsequent spark plasma sintering while ensuring that the powder is not oxidized. By controlling the ball milling parameters and sintering parameters, the size and distribution of La2O3 particles are controlled, and the mechanical properties of the refractory alloy are improved to varying degrees.
[0028] Compared with the conventional refractory alloy preparation method, the present invention has the following advantages:
[0029] 1. The present invention regulates the in-situ generation of La by regulating ball milling parameters and controlling spark plasma sintering parameters. 0.33 TaO3 and La 4.8 Ta 22 O 62 Size and distribution of two composite oxide particles.
[0030] 2. Aggregated La2O3 particles are enriched at the grain boundaries as the second phase, filling part of the pores and improving the density of the refractory alloy. The mechanical properties of the refractory alloy can also be improved through the second phase strengthening mechanism. The complex oxides formed at the grain boundaries and the matrix play a role in absorbing oxygen to a certain extent. While ensuring other properties, the strength and toughness are better than those of the refractory alloy prepared by conventional methods.
[0031] 3. CN117802384A improves toughness by adding Si element, and the plasticity can reach 6%. The plasticity of this method exceeds 10%, and the best can reach 22%. Compared with patent CN109182877A, not only the plasticity is significantly improved, but also the strength is increased by about 300MPa.
[0032] In summary, the method adopted in the present invention is simple and convenient. The prepared refractory alloy has better properties such as density and strength than those prepared by conventional methods while maintaining high toughness, and has the prospect of industrial-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a STEM-HAADF image of the product obtained in Example 2;
[0034] from Figure 1 It can be seen that La 0.33 TaO3 and La 4.8 Ta 22 O 62 The particle sizes of the two composite oxides are 300-500nm and are dispersed at the grain boundaries. DETAILED DESCRIPTION
[0035] Example 1
[0036] Step 1: Mixing of raw material element powder and powder
[0037] According to the designed powder ratio of each component element and the required La2O3 powder ratio, 8.62g of Mo powder (particle size is 1μm), 8.35g of Nb powder (particle size is 1μm), 16.26g of Ta powder (particle size is 1μm), 16.52g of W powder (particle size is 1μm), and 0.239g of La2O3 powder (particle size is 500nm) are weighed, and each raw material powder is placed in a ball mill, with a ball-to-material mass ratio of 10:1 (grinding ball diameter is 5-8mm), a ball milling speed of 250 rpm, and under argon protection, four steps of forward rotation → stop → reverse rotation → stop are followed, each step is repeated for 30 minutes, and the ball mill is performed for 30 hours. The obtained powder is sieved through a 40mm sieve, and the sieve-under material is taken to obtain the final powder mixture.
[0038] Step 2: Preparation of MoNbTaW-La2O3 refractory alloy bulk
[0039] The uniformly mixed refractory alloy powder obtained in the first step is made into a block by spark plasma sintering. The sintering pressure is 40MPa and the vacuum conditions are: the gas pressure in the furnace is less than 200Pa. It is heated to 1600°C at a heating rate of 80°C / min and kept warm for 10 minutes. It is cooled with the furnace to obtain a MoNbTaW-La2O3 refractory alloy block.
[0040] The refractory alloy material prepared in this example has a yield strength of 1700 MPa and a fracture strain of 15% when compressed at room temperature.
[0041] Example 2
[0042] Step 1: Preparation of MoNbTaW-La2O3 refractory alloy powder
[0043] According to the designed powder ratio of each component element and the required La2O3 powder ratio, 8.62g of Mo powder (particle size is 1μm), 8.35g of Nb powder (particle size is 1μm), 16.26g of Ta powder (particle size is 1μm), 16.52g of W powder (particle size is 1μm), and 0.239g of La2O3 powder (particle size is 500nm) are weighed. Each raw material powder is placed in a ball mill, with a ball-to-material mass ratio of 10:1 (the diameter of the grinding ball is 5-8mm), a ball milling speed of 350 rpm, and under argon protection, four steps of forward rotation → stop → reverse rotation → stop are followed, each step is repeated for 30 minutes, and the ball mill is performed for 40 hours. The obtained powder is sieved through a 40mm sieve, and the sieve under is taken to obtain the final powder mixture.
[0044] Step 2: Preparation of MoNbTaW-La2O3 refractory alloy bulk
[0045] The uniformly mixed refractory alloy powder obtained in the first step is made into a block by spark plasma sintering. The sintering pressure is 40MPa and the vacuum conditions are: the gas pressure in the furnace is less than 200Pa. It is heated to 2000°C at a heating rate of 80°C / min and kept warm for 10 minutes. It is cooled with the furnace to obtain a MoNbTaW-La2O3 refractory alloy block.
[0046] The refractory alloy material prepared in this example has a yield strength of 1750 MPa and a fracture strain of 30% when compressed at room temperature.
[0047] Example 3
[0048] Step 1: Preparation of MoNbTaW-La2O3 refractory alloy powder
[0049] According to the designed powder ratio of each component element and the required La2O3 powder ratio, 8.62g of Mo powder (particle size is 1μm), 8.35g of Nb powder (particle size is 1μm), 16.26g of Ta powder (particle size is 1μm), 16.52g of W powder (particle size is 1μm), and 0.239g of La2O3 powder (particle size is 500nm) are weighed, and each raw material powder is placed in a ball mill, with a ball-to-material mass ratio of 10:1 (the diameter of the grinding ball is 5-8mm), a ball milling speed of 250 rpm, and under argon protection, four steps of forward rotation → stop → reverse rotation → stop are followed, each step is repeated for 30 minutes, and the ball mill is performed for 30 hours. The obtained powder is sieved through a 40mm sieve, and the sieve under is taken to obtain the final powder mixture.
[0050] Step 2: Preparation of MoNbTaW-La2O3 refractory alloy bulk
[0051] The uniformly mixed refractory alloy powder obtained in the first step is made into a block by spark plasma sintering. The sintering pressure is 40MPa and the vacuum conditions are: the gas pressure in the furnace is less than 200Pa. It is heated to 1800°C at a heating rate of 80°C / min and kept warm for 10 minutes. It is cooled with the furnace to obtain a MoNbTaW-La2O3 refractory alloy block.
[0052] The refractory alloy material prepared in this example has a yield strength of 1700 MPa and a fracture strain of 19% when compressed at room temperature.
[0053] Example 4
[0054] Step 1: Preparation of MoNbTaW-La2O3 refractory alloy powder
[0055] According to the designed powder ratio of each component element and the required La2O3 powder ratio, 8.62g of Mo powder (particle size is 1μm), 8.35g of Nb powder (particle size is 1μm), 16.26g of Ta powder (particle size is 1μm), 16.52g of W powder (particle size is 1μm), and 0.239g of La2O3 powder (particle size is 500nm) are weighed, and each raw material powder is placed in a ball mill, with a ball-to-material mass ratio of 10:1 (the diameter of the grinding ball is 5-8mm), a ball milling speed of 250 rpm, and under argon protection, four steps of forward rotation → stop → reverse rotation → stop are followed, each step is repeated for 30 minutes, and the ball mill is performed for 30 hours. The obtained powder is sieved through a 40mm sieve, and the sieve under is taken to obtain the final powder mixture.
[0056] Step 2: Preparation of MoNbTaW-La2O3 refractory alloy bulk
[0057] The uniformly mixed refractory alloy powder obtained in the first step is made into a block by spark plasma sintering. The sintering pressure is 40MPa and the vacuum condition is 200Pa or less. It is heated to 2100°C at a heating rate of 80°C / min and kept warm for 10 minutes. It is cooled in the furnace to obtain a MoNbTaW-La2O3 refractory alloy block.
[0058] The precipitates in the refractory alloy material prepared in this example are reduced, but the grains are significantly enlarged, the yield strength during compression at room temperature is 1500 MPa, and the fracture strain is 19%.
[0059] Example 5
[0060] Step 1: Preparation of MoNbTaW-La2O3 refractory alloy powder
[0061] According to the designed powder ratio of each component element and the required La2O3 powder ratio, 8.62g of Mo powder (particle size is 1μm), 8.35g of Nb powder (particle size is 1μm), 16.26g of Ta powder (particle size is 1μm), 16.52g of W powder (particle size is 1μm), and 0.239g of La2O3 powder (particle size is 500nm) are weighed, and each raw material powder is placed in a ball mill, with a ball-to-material mass ratio of 10:1 (the diameter of the grinding ball is 5-8mm), a ball milling speed of 350 rpm, and under argon protection, four steps of forward rotation → stop → reverse rotation → stop are followed, each step is repeated for 30 minutes, and the ball mill is performed for 50 hours. The obtained powder is sieved through a 40mm sieve, and the sieve under is taken to obtain the final powder mixture.
[0062] Step 2: Preparation of MoNbTaW-La2O3 refractory alloy bulk
[0063] The uniformly mixed refractory alloy powder obtained in the first step is made into a block by spark plasma sintering. The sintering pressure is 40MPa. The vacuum condition is that the pressure in the furnace is less than 200Pa. It is heated to 2000℃ at a heating rate of 80℃ / min and kept warm for 10 minutes. It is cooled with the furnace to obtain a MoNbTaW-La2O3 refractory alloy block.
[0064] The refractory alloy material prepared in this example has a yield strength of 1600 MPa and a fracture strain of 18% when compressed at room temperature.
[0065] Example 6
[0066] The other conditions were the same as those in Example 2, except that: the amount of La2O3 powder added was 1% by mass;
[0067] The yield strength of the obtained product during compression at room temperature is 1700 MPa and the fracture strain is 24%.
[0068] Example 7
[0069] The other conditions were the same as those in Example 2, except that: the amount of La2O3 powder added was 1.5% by mass;
[0070] The yield strength of the obtained product during compression at room temperature is 1750 MPa and the fracture strain is 20%.
[0071] Comparative Example 1
[0072] The other conditions were the same as those in Example 2, except that La2O3 powder was not added;
[0073] The yield strength of the obtained product during compression at room temperature is 1200 MPa and the fracture strain is 13%.
[0074] Comparative Example 2
[0075] The other conditions were the same as those in Example 1, except that La2O3 powder was not added;
[0076] The yield strength of the obtained product during compression at room temperature is 1000 MPa and the fracture strain is 10%.
Claims
1. A high-strength and tough refractory alloy, characterized in that: The refractory alloy comprises a refractory alloy matrix and La dispersed in the refractory alloy matrix. 0.33 TaO3 and La 4.8 Ta 22 O 62 Two kinds of composite oxide particles; La 0.33 TaO3 and La 4.8 Ta 22 O 62 The size of the two composite oxide particles is less than 600nm, and they are dispersed at the grain boundaries; La 0.33 TaO3 and La 4.8 Ta 22 O 62 The total molar amount of the two composite oxide particles accounts for 0.1-1 at% of the refractory alloy, preferably 0.4-0.6 at%; the refractory alloy matrix is composed of four elements: Nb, Mo, W and Ta.
2. A high strength and toughness refractory alloy according to claim 1, characterized in that: The atomic percentage of any transition metal element in the refractory alloy matrix is 24.5-25.5 at.%.
3. A method for preparing a high-strength and tough refractory alloy according to any one of claims 1 to 2, characterized in that: Transition metal element powder and La2O3 powder are prepared according to the designed proportion, and a mixed powder is obtained by high-energy ball milling. The refractory alloy mixed powder after high-energy ball milling is then subjected to discharge plasma sintering to obtain a high-strength and tough refractory alloy material; the average particle size of the transition metal element powder is less than or equal to 10μm, and the average particle size of La2O3 is less than or equal to 2μm; in the mixed powder, the mass fraction of La2O3 is 0.2-1.5%.
4. The method for preparing a high-strength and tough refractory alloy according to claim 3, characterized in that: In the mixed powder, the mass fraction of La2O3 is 0.4-0.6%.
5. The method for preparing a high-strength and tough refractory alloy according to claim 3, characterized in that: The average particle size of the transition metal element powder is 0.5-10 μm, and the average particle size of La2O3 is 0.1-2 μm.
6. The method for preparing a high-strength and tough refractory alloy according to claim 3, characterized in that: The parameters of the high-energy ball milling are: a ball-to-material mass ratio of 9 to 11:1, a ball milling speed of 200 to 400 rpm, and a ball milling time of 20 to 50 h, preferably 28 to 42 h.
7. The method for preparing a high-strength and tough refractory alloy according to claim 3, characterized in that: The high energy ball milling is dry ball milling.
8. The method for preparing a high-strength and tough refractory alloy according to claim 6, characterized in that: During high-energy ball milling, forward and reverse alternating ball milling is adopted, and the process is carried out in a cycle of forward rotation-stop-reverse rotation-stop. The time for any forward rotation, stop, reverse rotation, and stop is 20 to 30 minutes.
9. The method for preparing a high-strength and tough refractory alloy according to claim 3, characterized in that: The spark plasma sintering is carried out under vacuum conditions. The process of spark plasma sintering is: heating to 1600-2100°C, preferably 1800-2000°C, at a heating rate of 80-120°C / min, keeping the temperature for 8-15 minutes, and cooling to room temperature. The pressure of the spark plasma sintering is 30-50MPa.
10. The method for preparing a high-strength and tough refractory alloy according to claim 3, characterized in that: The ball-to-material mass ratio is 10:1; the ball milling speed is 350 revolutions per minute; the process is carried out in a cycle of forward rotation-stop-reverse rotation-stop, each step is carried out in a cycle of 30 minutes, and the ball milling is carried out for 40 hours to obtain a powder mixture; in terms of mass percentage, when the powder mixture contains 17.2-17.6% Mo, 16.5-17.1% Nb, 32.5-33.2% Ta, 33-33.7% W, and the balance is La2O3, The powder mixture was made into a block by spark plasma sintering, with a sintering pressure of 40MPa, vacuum conditions, and heated to 2000℃ at a heating rate of 80℃ / min, and kept at this temperature for 10 minutes, and then cooled with the furnace to obtain a MoNbTaW-La2O3 refractory alloy block. The room temperature compressive yield strength of the obtained MoNbTaW-La2O3 refractory alloy block was 1750MPa, and the fracture strain was 30%.