Supported noble metal catalyst as well as preparation method and application thereof

By loading 1-2 nm palladium clusters onto a NiFe2O4 support, the problems of poisoning and failure of noble metal catalysts and low efficiency of non-noble metal catalysts were solved, and efficient catalytic oxidation of VOCs at low temperatures was achieved.

CN118892847APending Publication Date: 2024-11-05SHAANXI ZHONGCHUANG NAT NEW MATERIAL TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410937776.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing precious metal catalysts are prone to poisoning and failure due to high-temperature sintering, while non-precious metal catalysts have low efficiency and most catalysts have high reaction window temperatures.

Method used

A supported noble metal catalyst was used, in which palladium clusters with a size of 1-2 nm were loaded on a NiFe2O4 support, and the relevant reaction conditions were controlled to improve the interaction between the metal and the support and enhance the catalytic activity.

Benefits of technology

The temperature window of the catalytic oxidation reaction was reduced, and the thermal stability and mechanical strength of the catalyst were improved, enabling effective catalytic oxidation of VOCs at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892847A_ABST
    Figure CN118892847A_ABST
Patent Text Reader

Abstract

The invention discloses a supported noble metal catalyst as well as a preparation method and application thereof, and relates to the field of nano catalyst preparation, the core of the supported noble metal catalyst is that the change of interaction between metal and a carrier is caused by regulating and controlling related reaction conditions, the electron transfer between metal palladium and the carrier NiFe2O4 at an interface is improved, and the catalytic activity of the catalyst is improved. Palladium clusters are rich in electrons to activate oxygen, and the carrier is deficient in electrons to adsorb toluene. Wherein the granularity of palladium clusters formed on the surface of the prepared catalyst carrier is smaller and is 1-2nm, so that the catalyst carrier has higher specific surface area and active site density. The palladium cluster can be more effectively contacted with molecular oxygen in the air and activated, so that the catalytic activity of the catalyst is improved. Besides, NiFe2O4 serving as a carrier has good thermal stability and mechanical strength, provides a stable supporting environment for palladium clusters, facilitates uniform dispersion of palladium and plays an important role in the interface electron transfer process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano catalyst development and relates to a supported noble metal catalyst and a preparation method and application thereof. Background Art

[0002] Volatile Organic Compounds (VOCs) are an important component of air pollutants. They play an important role in the formation of smog-related ozone and photochemical oxidants. In addition, VOCs are also extremely harmful to human health. They can cause headaches, vomiting or fatigue at the mildest, and cancer, deformity and even death at the worst. Therefore, the control of VOCs emissions has attracted widespread attention. With the advancement of science and technology and the continuous improvement of environmental protection requirements, VOCs treatment technology is also developing and innovating. Among the many treatment technologies, catalytic oxidation technology is one of the more promising technologies at present. It uses the action of catalysts to make VOCs and oxygen undergo oxidation reaction at a certain temperature to generate harmless substances such as carbon dioxide and water. Common catalysts mainly include precious metal catalysts and non-precious metal oxide catalysts. Precious metal catalysts, such as those containing platinum, palladium and gold, are widely favored because of their high efficiency. However, these catalysts are easily deactivated by high-temperature sintering or poisoning, and are expensive. Although non-precious metal oxide catalysts are cheap and have strong resistance to poisoning, they are not as durable as precious metal catalysts and have low efficiency. In addition, the reaction windows of most catalysts currently used for catalytic oxidation removal of VOCs are mostly above 200°C, and the required reaction temperature is relatively high. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention provides a supported precious metal catalyst and a preparation method and application thereof, thereby solving the technical problems in the prior art that precious metal catalysts in VOCs catalytic oxidation materials are easily sintered and poisoned to become ineffective, non-precious metal catalysts are inefficient, and the reaction window temperature of most catalysts is relatively high.

[0004] The present invention is achieved through the following technical solutions:

[0005] A supported noble metal catalyst comprises a NiFe2O4 carrier on which palladium clusters are supported; the size of the palladium clusters is 1-2 nm.

[0006] The above-mentioned method for preparing a supported noble metal catalyst comprises the following steps:

[0007] S1: dispersing a nickel precursor and an iron precursor in ethylene glycol to obtain a precursor mixed solution, then adding a precipitant solution to the precursor mixed solution, stirring the mixture to react, centrifuging, washing, drying, and then calcining the obtained product to obtain a NiFe2O4 carrier;

[0008] S2: dispersing the palladium precursor solution into the suspension of the NiFe2O4 carrier, heating and stirring to react, centrifuging, washing and drying the obtained product, performing a heat treatment, and then performing a second heat treatment in a reducing atmosphere to obtain the supported precious metal catalyst.

[0009] Preferably, the molar ratio of the nickel precursor, the iron precursor and the precipitant is (0.001-2.0):(0.001-2.0):(0.001-2.0).

[0010] Preferably, in step S1, the nickel precursor is at least one of nickel nitrate, nickel chloride and nickel acetate; the iron precursor is at least one of ferric nitrate, ferric chloride, ferric acetate and ferric sulfate; the precipitant is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, oxalic acid, ammonium carbonate and ammonium bicarbonate.

[0011] Preferably, in step S1, the calcination temperature is 300-800°C, the calcination time is 2-6 hours, and the heating rate is 1-20°C / min.

[0012] Preferably, in step S2, the palladium precursor is at least one of sodium tetrachloropalladate, potassium tetrachloropalladate, potassium hexachloropalladate, palladium nitrate and tetraamminepalladium nitrate.

[0013] Preferably, in step S2, the palladium precursor solution is dispersed into the suspension of the NiFe2O4 carrier and heated and stirred. Specifically, 5 to 30 mL of a palladium precursor liquid solution with a concentration of 0.001 to 0.2 mol / L is dispersed into 10 to 100 mL of a suspension containing 0.1 to 3 g of a NiFe2O4 carrier, and stirring is continued at 45 to 95°C for 2 to 8 hours.

[0014] Preferably, in step S2, the atmosphere of the primary heat treatment is air, helium or nitrogen; the temperature of the primary heat treatment is 100-600°C, the time is 0.5-5h, and the heating rate is 1-20°C / min.

[0015] Preferably, in step S2, the reducing atmosphere is carbon monoxide, hydrogen or ammonia; the temperature of the secondary heat treatment is 100-600°C, the time is 0.5-5h, and the heating rate is 1-20°C / min.

[0016] The above-mentioned application of a supported precious metal catalyst in VOCs thermal catalysis.

[0017] Compared with the prior art, the present invention has the following beneficial technical effects:

[0018] The present invention discloses a supported precious metal catalyst, the core of which is to highly and evenly load palladium clusters with a size of 1 to 2 nm on a NiFe2O4 carrier to form a supported precious metal catalyst. In the preparation of the material, the interaction between the metal and the carrier is changed by regulating the relevant reaction conditions, thereby improving the electron transfer between the metal palladium and the carrier NiFe2O4 at the interface, the palladium clusters are rich in electrons to activate oxygen, and the carrier is electron-deficient to adsorb toluene. Among them, since the particle size of the palladium clusters formed on the surface of the prepared catalyst carrier is 1 to 2 nm, it has a higher specific surface area and active site density, which enables the palladium clusters to more effectively contact and activate molecular oxygen in the air, thereby improving the catalytic activity of the catalyst. Because in the catalytic oxidation process of VOCs, precious metals play a vital role in the adsorption and activation of molecular oxygen. In the present invention, gas-phase molecular oxygen is adsorbed on the surface of the palladium cluster and activated into oxygen atoms, and then the adsorbed toluene molecules are further oxidized by the active oxygen atoms to eventually generate carbon dioxide and water. In addition, the spinel-type composite metal oxide NiFe2O4 used as a carrier in the present invention has good thermal stability and mechanical strength. It provides a stable supporting environment for palladium clusters, which is not only conducive to the uniform dispersion of palladium, but also plays an important role in the interfacial electron transfer process, and avoids the agglomeration, sintering and deactivation of precious metal catalysts in the VOCs thermal catalytic process. At the same time, due to the improvement of catalytic performance, the temperature window of the catalytic oxidation reaction is effectively reduced.

[0019] In addition, the present invention also discloses a method for preparing the above-mentioned supported noble metal catalyst, which first disperses a nickel precursor and an iron precursor into ethylene glycol, and adds a precipitant solution for stirring reaction, so that the formation process of the NiFe2O4 carrier can be accurately controlled. Ethylene glycol, as a solvent, is conducive to the uniform dispersion and reaction of the precursor, thereby obtaining a spinel-type composite metal oxide NiFe2O4 carrier with uniform structure and stable performance. Then, the palladium precursor solution is dispersed into the suspension of the NiFe2O4 carrier, and the obtained product is centrifuged, washed and dried by heating and stirring, and then subjected to a heat treatment, and then subjected to a secondary heat treatment in a reducing atmosphere, effectively causing changes in the interaction between the metal and the carrier, improving the electron transfer between the metal palladium and the carrier NiFe2O4 at the interface, and finally improving the catalytic activity of the catalyst. In this process, heating and stirring are conducive to promoting the combination between the palladium precursor and the carrier. After the primary heat treatment, a secondary heat treatment is performed in a reducing atmosphere. This step is crucial to the performance of the catalyst. The primary heat treatment not only helps to remove impurities, moisture and organic residues on the surface of the carrier, but also can significantly increase the interaction strength between the metal palladium and the carrier NiFe2O4, providing conditions for changes in the interface characteristics between the metal and the carrier. The secondary heat treatment in a reducing atmosphere is mainly to promote the reduction of high-valent palladium on the surface of the carrier NiFe2O4 to a low-valent state, because low-valent palladium helps the adsorption and activation of molecular oxygen. Therefore, this process promotes the ability of the catalytic material to catalytically oxidize toluene at low temperatures, thereby reducing the temperature window for the catalytic oxidation reaction of toluene. In addition, the catalyst also has good thermal stability and mechanical strength, and can maintain stable catalytic performance during long-term use.

[0020] Further, the molar ratio of the nickel precursor, the iron precursor and the precipitant is (0.001-2.0):(0.001-2.0):(0.001-2.0). By adjusting the molar ratio of the nickel precursor to the iron precursor, the ratio of nickel and iron in the NiFe2O4 carrier can be accurately controlled, thereby obtaining a spinel-type composite metal oxide NiFe2O4 carrier with different metal elements. As is well known, a spinel-type composite metal oxide refers to a metal oxide with a spinel structure, in which the A position and the B position can be occupied by different metal ions to form a material with multiple functions. These materials usually have a chemical formula of AB2O4, but the actual chemical composition may be more complex, because the A position and the B position can be occupied by a variety of metal ions to form a solid solution. In the present invention, nickel and iron play different roles in the NiFe2O4 carrier, nickel has better catalytic activity, and iron helps to enhance the stability and mechanical strength of the catalyst. By adjusting the ratio of nickel and iron, the activity, stability and mechanical strength of the catalyst can be balanced, resulting in a catalyst with excellent comprehensive performance.

[0021] Further, in step S1, the calcination temperature is 300-800°C, the calcination time is 2-6h, and the heating rate is 1-20°C / min. Calcination within this temperature range is conducive to the crystallization and phase change of the NiFe2O4 carrier, thereby obtaining a carrier with a more stable structure and better performance. Appropriate calcination temperature and time can promote the crystallization of the carrier, reduce amorphous substances, and improve the crystallinity and purity of the carrier. The control of calcination temperature and time has a direct effect on the size of the metal particles. Excessive temperature or too long time may cause the agglomeration and enlargement of the metal particles, affecting the activity of the catalyst. At a calcination temperature of 300-800°C, combined with a calcination time of 2-6 hours and a heating rate of 1-20°C / min, the size of the metal particles can be effectively controlled to keep it at the nanometer level, thereby improving the activity of the catalyst. Appropriate calcination treatment can remove impurities and organic matter on the surface of the carrier, increase the specific surface area and the number of active sites of the carrier. After calcination, the surface of the carrier is cleaner, which is conducive to the subsequent uniform loading of palladium and the formation of small-sized palladium clusters. Calcination treatment can also improve the thermal stability and mechanical strength of the carrier, so that it can maintain stable catalytic performance under harsh conditions such as high temperature and high pressure. The stable carrier structure can ensure the firm loading of the palladium cluster on the carrier and prevent the catalyst from falling off or deactivating during use. Therefore, in step S1, setting the calcination temperature to 300-800°C, the calcination time to 2-6 hours, and the heating rate to 1-20°C / min can optimize the carrier structure, control the size of metal particles, enhance the catalytic activity, and improve the stability of the catalyst.

[0022] Further, in step S2, the palladium precursor solution is dispersed into the suspension of the NiFe2O4 carrier, heated and stirred, specifically: 5-30 mL of a palladium precursor liquid solution with a concentration of 0.001-0.2 mol / L is dispersed into 10-100 mL of a NiFe2O4 carrier suspension containing 0.1-3 g, and stirred continuously at 45-95 ° C for 2-8 hours. By controlling the volume and concentration of the palladium precursor solution, as well as the mass and suspension volume of the NiFe2O4 carrier, the loading amount of the palladium cluster on the carrier can be accurately controlled. Appropriate loading is essential for the activity of the catalyst. Too much palladium may lead to waste and easily cause the agglomerated particles to increase in size, while too little may not be enough to provide enough catalytic active sites. Dispersing the palladium precursor solution into the suspension of the NiFe2O4 carrier helps to uniformly disperse the palladium cluster on the carrier. Uniform dispersibility can ensure that the active sites of the palladium cluster on the carrier are evenly distributed, thereby improving the catalytic efficiency and stability of the catalyst. The NiFe2O4 carrier in the suspension provides a large number of surfaces and pores, which can serve as attachment points for palladium clusters. When the palladium precursor solution is mixed with the carrier suspension, the palladium ions can bind to the carrier surface through adsorption and other methods to form a stable palladium precursor-NiFe2O4 system. This method can effectively enhance the bonding between the palladium precursor and the carrier and prevent the palladium precursor from being free in the solvent.

[0023] Furthermore, in step S2, the atmosphere of the primary heat treatment is air, helium or nitrogen; the temperature of the primary heat treatment is 100-600°C, the time is 0.5-5h, and the heating rate is 1-20°C / min. Appropriate primary heat treatment not only helps to remove impurities, moisture and organic residues on the surface of the carrier, but also can significantly improve the interaction strength between metal palladium and the carrier NiFe2O4, providing conditions for causing changes in the interface characteristics between the metal and the carrier.

[0024] Further, in step S2, the reducing atmosphere is carbon monoxide, hydrogen or ammonia, and carbon monoxide, hydrogen and ammonia are all reducible to the precious metal palladium, and they can effectively reduce the palladium precursor, i.e., the high-valent palladium, to low-valent palladium. This reduction process is crucial for preparing a highly active supported precious metal catalyst, because the low-valent palladium is the active center of the catalyst. By adjusting the concentration, flow rate and reduction temperature of the reducing atmosphere, the reduction degree of the palladium precursor can be accurately controlled. This helps to optimize the activity of the catalyst, because excessive reduction may cause the agglomeration of palladium particles, thereby reducing the activity of the catalyst. In a reducing atmosphere, metal palladium can be evenly dispersed on the NiFe2O4 carrier to form a stable palladium cluster. This uniform dispersibility helps to improve the catalytic efficiency and stability of the catalyst. Using carbon monoxide, hydrogen or ammonia as a reducing atmosphere is simple and easy to operate and easy to control. These gases can accurately adjust their flow and concentration through a flow meter and a control system to ensure the stability and repeatability of the reduction process. The temperature of the secondary heat treatment is 100-600°C, the time is 0.5-5h, and the heating rate is 1-20°C / min. Appropriate heat treatment in a reducing atmosphere can improve the electron transfer between the metal palladium and the carrier NiFe2O4 at the interface. The palladium cluster is rich in electrons to activate oxygen, and the carrier lacks electrons to adsorb toluene. Because low-valent palladium helps the adsorption and activation of molecular oxygen, this process promotes the ability of the catalytic material as a whole to catalytically oxidize toluene at low temperatures, thereby reducing the temperature window for the catalytic oxidation reaction of toluene. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 It is a schematic diagram of a process for preparing a supported noble metal catalyst in the present invention;

[0027] Figure 2 This is a high-angle annular dark field scanning transmission electron micrograph (HAADF-STEM) of a supported noble metal catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0030] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0031] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0032] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0033] like Figure 1 As shown, the present invention provides a method for preparing a supported noble metal catalyst, comprising the following steps:

[0034] S1: dispersing a nickel precursor and an iron precursor in ethylene glycol, then adding a precipitant solution to the above solution, stirring for reaction, centrifuging, washing, drying and calcining the obtained product to obtain a NiFe2O4 carrier;

[0035] Specifically, at room temperature, 0.001-2.0 mol of nickel precursor and 0.001-2.0 mol of iron precursor are dispersed in 20-200 mL of ethylene glycol, 20-200 mL of a newly prepared 0.01-2.0 mol / L precipitant solution is added to the above solution, and the solid precipitate obtained after stirring and reacting for 0.5-5 h is centrifuged, washed, dried at 60-100 ° C for 6-12 h, and calcined at 300-800 ° C for 2-6 h at a heating rate of 1-20 ° C / min, and the obtained product is the carrier NiFe2O4;

[0036] Among them, the nickel precursor is at least one of nickel nitrate, nickel chloride and nickel acetate; the iron precursor is at least one of iron nitrate, iron chloride, iron acetate and iron sulfate; the precipitant is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, oxalic acid, ammonium carbonate and ammonium bicarbonate.

[0037] In step S1, the drying temperature is 60-100°C, and the drying time is 6-12h. The drying process can effectively remove the residual ethylene glycol or other solvents in the product. These residual solvents will affect the loading of the palladium clusters and the performance of the catalyst in the subsequent steps. Appropriate drying temperature and time can ensure that the solvent is fully removed to obtain a pure NiFe2O4 carrier. At a drying temperature of 60-100°C, the structure of the NiFe2O4 carrier can be effectively maintained to avoid structural damage or phase change caused by high temperature. Appropriate drying temperature and time help to maintain the pore structure and specific surface area of ​​the carrier, which is crucial for the subsequent loading of palladium clusters and the activity of the catalyst. The dried NiFe2O4 carrier has better adsorption properties and can more effectively adsorb palladium ions in the palladium precursor solution. This helps to improve the loading efficiency and distribution uniformity of palladium clusters on the carrier, thereby enhancing the catalytic performance of the catalyst. The selection of drying temperature and time takes into account the balance between cost and efficiency. The temperature range of 60-100°C is relatively low, which can save energy costs. At the same time, 6 to 12 hours can effectively remove residual solvents, maintain carrier structure, improve loading efficiency, control drying costs and ensure product quality.

[0038] S2: dispersing the palladium precursor solution into the suspension of the NiFe2O4 carrier, heating and stirring to react, centrifuging, washing and drying the obtained product, performing a heat treatment, and then performing a second heat treatment in a reducing atmosphere to obtain the supported precious metal catalyst.

[0039] Specifically, 0.1-3 g of carrier NiFe2O4 is dispersed in 10-100 mL of deionized water, 5-30 mL of a newly prepared 0.001-0.2 mol / L palladium precursor liquid solution is dispersed in the suspension of carrier NiFe2O4, and the solid precipitate is centrifuged after continuous stirring at 45-95°C for 2-8 hours, washed, and dried at 60-100°C for 6-12 hours, and firstly heat-treated at 100-600°C for 0.5-5 hours with a heating rate of 1-20°C / min; and then heat-treated at 100-600°C in a reducing atmosphere for 0.5-5 hours with a heating rate of 1-20°C / min. The obtained product is the target catalyst.

[0040] The palladium precursor liquid is at least one of sodium tetrachloropalladate, potassium tetrachloropalladate, potassium hexachloropalladate, palladium nitrate and tetraammine palladium nitrate. The primary heat treatment atmosphere is air, helium or nitrogen, and the reducing atmosphere, i.e., the atmosphere of the secondary heat treatment, is carbon monoxide, hydrogen or ammonia.

[0041] The present invention also discloses a supported noble metal catalyst obtained by the above method. The supported noble metal catalyst comprises a NiFe2O4 carrier, on which palladium clusters are highly uniformly supported. The size of the palladium clusters is 1 to 2 nm.

[0042] When the supported noble metal catalyst prepared in the present invention is used for thermal catalytic oxidation of VOCs, the reaction window of catalytic oxidation of toluene is lower than 200°C.

[0043] The supported precious metal catalyst prepared by the present invention uses spinel composite metal oxide NiFe2O4 as a carrier, and the active component precious metal palladium is highly and evenly distributed on the carrier in the form of clusters, which solves the problems of high cost of precious metal catalysts, low efficiency of non-precious metal catalysts, and high reaction window temperature of most catalysts. The size of the palladium cluster supported on NiFe2O4 in the supported precious metal catalyst prepared by the present invention is 1 to 2 nm. The over-regulation of relevant reaction conditions in the material preparation causes changes in the interaction between the metal and the carrier, improves the electron transfer between the metal palladium and the carrier NiFe2O4 at the interface, the palladium cluster is rich in electrons to activate oxygen, and the carrier lacks electrons to adsorb toluene, which promotes the system's ability to catalyze the oxidation of toluene, and finally reduces the temperature window during the catalytic oxidation reaction of toluene. The preparation method provided in the present invention is simple, the process is controllable, and has good practical application prospects.

[0044] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0045] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0046] Example 1

[0047] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0048] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.1 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0049] Example 2

[0050] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L sodium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The obtained solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0051] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.1 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0052] Example 3

[0053] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L oxalic acid solution was added to the above solution, and the reaction was stirred for 3 h. The obtained solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0054] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.1 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0055] Example 4

[0056] (1) At room temperature, 0.001 mol nickel nitrate and 0.002 mol iron nitrate were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The obtained solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0057] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.1 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0058] Example 5

[0059] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The obtained solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 300 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0060] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.1 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0061] Example 6

[0062] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0063] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.001 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0064] Example 7

[0065] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0066] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a freshly prepared 0.2 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. Thereafter, it was treated in nitrogen at 500°C for 3 h, and then in a carbon monoxide atmosphere at 300°C for 2 h, with a heating rate of 20°C / min. The obtained product was the target catalyst.

[0067] Example 8

[0068] (1) At room temperature, 0.001 mol nickel chloride and 0.002 mol ferric chloride were dispersed in 50 mL ethylene glycol, 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution, and the reaction was stirred for 3 h. The solid precipitate was centrifuged, washed, dried at 100 ° C for 12 h, and calcined at 700 ° C for 5 h at a heating rate of 20 ° C / min. The obtained product was the carrier NiFe2O4;

[0069] (2) 0.5 g of carrier NiFe2O4 was dispersed in 50 mL of deionized water, and 20 mL of a newly prepared 0.1 mol / L chloropalladic acid solution was dispersed in the suspension of carrier NiFe2O4. After continuous stirring at 80°C for 3 h, the obtained solid precipitate was centrifuged, washed, and dried at 100°C for 12 h. After that, it was first treated in helium at 500°C for 3 h, and then treated in an ammonia atmosphere at 300°C for 2 h, with a heating rate of 20°C / min.

[0070] The obtained product is the target catalyst.

[0071] Comparative Example

[0072] At room temperature, 0.001 mol of nickel chloride and 0.002 mol of ferric chloride were dispersed in 50 mL of ethylene glycol, and 50 mL of a newly prepared 2.0 mol / L ammonium carbonate solution was added to the above solution. After stirring for 3 hours, the obtained solid precipitate was centrifuged, washed, dried at 100°C for 12 hours, and calcined at 700°C for 5 hours at a heating rate of 20°C / min. The obtained product was the carrier NiFe2O4.

[0073] In order to compare the performance of the catalysts prepared in the above Examples 1 to 8 and the comparative example, the prepared catalytic material was used to catalytically oxidize toluene. In the test process, a 30-60 mesh catalyst was weighed and filled into a fixed bed reactor. Toluene with an initial concentration of 100 ppm, a gas flow rate of 100 mL / min, and a space velocity of 60000 mL / (g·h) was introduced into the fixed bed reactor. The temperatures (denoted as T ) required when the toluene conversion rates were 10%, 50%, and 90% were measured. 10 、T 50 、T 90 ) The effect of the catalyst on catalytic oxidation of toluene was evaluated. The test results are shown in Table 1. As can be seen from Table 1, the thermal catalytic reaction window of the supported noble metal catalyst obtained in the present invention is less than 200°C.

[0074] Table 1 Comparison of catalytic temperature windows of the catalysts prepared in the above Examples 1 to 8 and the comparative examples

[0075] serial number <![CDATA[T 10 ]]> <![CDATA[T 50 ]]> <![CDATA[T 90 ]]> Example 1 155℃ 162℃ 171℃ Example 2 157℃ 165℃ 177℃ Example 3 146℃ 155℃ 165℃ Example 4 150℃ 160℃ 169℃ Example 5 153℃ 167℃ 172℃ Example 6 168℃ 179℃ 188℃ Example 7 140℃ 145℃ 155℃ Example 8 151℃ 165℃ 172℃ Comparative Example 190℃ 212℃ 230℃

[0076] in addition, Figure 2 This is a HAADF-STEM image of a supported precious metal catalyst prepared in Example 1 of the present invention. It can be seen from the image that the palladium on the surface of the NiFe2O4 carrier is about 1 nm in size and is evenly distributed.

[0077] In summary, the present invention provides a supported catalyst in which precious metal palladium is uniformly supported on NiFe2O4, wherein the precious metal palladium is highly and uniformly distributed on the carrier in the form of clusters with a size of about 1 to 2 nm. The catalyst is applied to the catalytic oxidation of VOCs, and the complete conversion of VOCs can be achieved at low temperature (below 200°C).

[0078] Example 9

[0079] A method for preparing a supported noble metal catalyst comprises the following steps:

[0080] S1: At room temperature, 0.001 mol of nickel precursor and 0.001 mol of iron precursor were dispersed in 20 mL of ethylene glycol, 0.001 mol of precipitant solution was added to the above solution, and the solid precipitate was obtained after stirring for 0.5 h, centrifuged, washed, dried at 60 ° C for 6 h, and calcined at 300 ° C for 6 h at a heating rate of 1 ° C / min. The obtained product is the carrier NiFe2O4;

[0081] Wherein, the nickel precursor is a mixture of nickel nitrate and nickel chloride; the iron precursor is a mixture of ferric nitrate, ferric chloride and ferric acetate; and the precipitant is sodium hydroxide.

[0082] S2: Disperse 0.1g of carrier NiFe2O4 into 10mL of deionized water to obtain a suspension of carrier NiFe2O4, take 5mL of newly prepared 0.001mol / L palladium precursor liquid solution and disperse it into the suspension of carrier NiFe2O4, stir continuously at 45°C for 2h, centrifuge the obtained solid precipitate, wash, dry at 60°C for 6h, heat treat once at 100°C for 5h, and then heat treat at 100°C in a reducing atmosphere for 5h with a heating rate of 1°C / min. The obtained product is the target catalyst.

[0083] The palladium precursor liquid is sodium tetrachloropalladate, potassium tetrachloropalladate and potassium hexachloropalladate. The primary heat treatment atmosphere is air, and the reducing atmosphere is carbon monoxide.

[0084] Example 10

[0085] A method for preparing a supported noble metal catalyst comprises the following steps:

[0086] S1: At room temperature, 2.0 mol of nickel precursor and 2.0 mol of iron precursor were dispersed in 200 mL of ethylene glycol, 2.0 mol of precipitant solution was added to the above solution, and the solid precipitate was obtained after stirring for 5 hours, centrifuged, washed, dried at 100°C for 12 hours, and calcined at 800°C for 2 hours at a heating rate of 20°C / min. The obtained product was the carrier NiFe2O4;

[0087] Wherein, the nickel precursor is nickel chloride and nickel acetate; the iron precursor is ferric sulfate; and the precipitant is ammonium carbonate and ammonium bicarbonate.

[0088] S2: Disperse 3 g of carrier NiFe2O4 into 100 mL of deionized water to obtain a suspension of carrier NiFe2O4, take 30 mL of a newly prepared 0.2 mol / L palladium precursor liquid solution and disperse it into the suspension of carrier NiFe2O4, stir continuously at 95°C for 8 h, centrifuge the obtained solid precipitate, wash, dry at 100°C for 6 h, heat treat once at 600°C for 0.5 h, and then heat treat at 600°C in a reducing atmosphere for 0.5 h, with a heating rate of 20°C / min. The obtained product is the target catalyst.

[0089] The palladium precursor liquid is palladium nitrate and tetraammine palladium nitrate. The primary heat treatment atmosphere is helium, and the reducing atmosphere is ammonia.

[0090] Embodiment 11

[0091] A method for preparing a supported noble metal catalyst comprises the following steps:

[0092] S1: At room temperature, 1 mol of nickel precursor and 1 mol of iron precursor were dispersed in 100 mL of ethylene glycol, 1 mol of precipitant solution was added to the above solution, and the solid precipitate was obtained after stirring for 3 hours, centrifuged, washed, dried at 80°C for 10 hours, and calcined at 500°C for 4 hours at a heating rate of 10°C / min. The obtained product was the carrier NiFe2O4;

[0093] Wherein, the nickel precursor is nickel acetate; the iron precursor is iron acetate; and the precipitant is sodium carbonate.

[0094] S2: Disperse 2 g of carrier NiFe2O4 in 50 mL of deionized water to obtain a suspension of carrier NiFe2O4, take 20 mL of a newly prepared 0.1 mol / L palladium precursor liquid solution and disperse it in the suspension of carrier NiFe2O4, stir continuously at 50°C for 6 h, centrifuge the obtained solid precipitate, wash, dry at 80°C for 10 h, heat treat at 300°C for 3 h, and then heat treat at 300°C in a reducing atmosphere for 3 h with a heating rate of 10°C / min. The obtained product is the target catalyst.

[0095] Wherein, the palladium precursor liquid is potassium hexachloropalladate, the primary heat treatment atmosphere is nitrogen, and the reducing atmosphere is hydrogen.

[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A supported noble metal catalyst, characterized in that: The invention comprises a NiFe2O4 carrier, on which palladium clusters are loaded; the size of the palladium clusters is 1-2nm.

2. The method for preparing a supported noble metal catalyst according to any one of claim 1, characterized in that: The following steps are involved: S1: dispersing a nickel precursor and an iron precursor in ethylene glycol to obtain a precursor mixed solution, then adding a precipitant solution to the precursor mixed solution, stirring the mixture to react, centrifuging, washing, drying, and then calcining the obtained product to obtain a NiFe2O4 carrier; S2: dispersing the palladium precursor solution into the suspension of the NiFe2O4 carrier, heating and stirring to react, centrifuging, washing and drying the obtained product, performing a heat treatment, and then performing a second heat treatment in a reducing atmosphere to obtain the supported precious metal catalyst.

3. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: The molar ratio of the nickel precursor, the iron precursor and the precipitant is (0.001-2.0):(0.001-2.0):(0.001-2.0).

4. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: In step S1, the nickel precursor is at least one of nickel nitrate, nickel chloride and nickel acetate; the iron precursor is at least one of ferric nitrate, ferric chloride, ferric acetate and ferric sulfate; the precipitant is at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, oxalic acid, ammonium carbonate and ammonium bicarbonate.

5. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: In step S1, the calcination temperature is 300-800°C, the calcination time is 2-6h, and the heating rate is 1-20°C / min.

6. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: In step S2, the palladium precursor is at least one of sodium tetrachloropalladate, potassium tetrachloropalladate, potassium hexachloropalladate, palladium nitrate and tetraamminepalladium nitrate.

7. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: In step S2, the palladium precursor solution is dispersed into the suspension of the NiFe2O4 carrier and heated and stirred. Specifically, 5 to 30 mL of a palladium precursor liquid solution with a concentration of 0.001 to 0.2 mol / L is dispersed into 10 to 100 mL of a suspension containing 0.1 to 3 g of a NiFe2O4 carrier, and stirring is continued at 45 to 95°C for 2 to 8 hours.

8. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: In step S2, the atmosphere of the primary heat treatment is air, helium or nitrogen; the temperature of the primary heat treatment is 100-600°C, the time is 0.5-5h, and the heating rate is 1-20°C / min.

9. The method for preparing a supported noble metal catalyst according to claim 2, characterized in that: In step S2, the reducing atmosphere is carbon monoxide, hydrogen or ammonia; the temperature of the secondary heat treatment is 100-600°C, the time is 0.5-5h, and the heating rate is 1-20°C / min.

10. Use of a supported noble metal catalyst as claimed in claim 1 in VOCs thermal catalysis.

Citation Information

Patent Citations

  • Catalyst for catalytic removal of carbon monoxide and formaldehyde under conditions of ambient temperature and humidity and preparation method of catalyst

    CN106391007A

  • Nano spinel type catalyst and preparation method thereof

    CN106622241A

  • Supported palladium catalyst using palladium oxide as support and preparation method thereof

    CN107456965A

  • Cobalt aluminate spinel loaded Pd-Pt catalyst and preparation method and application thereof

    CN113117694A

  • High-stability cerium oxide loaded palladium nanocluster catalytic material as well as preparation method and application thereof

    CN113769738A