Method for deep de-ashing and upgrading of coking coal slime
By performing oil agglomeration and selective flocculation treatment on coking coal slime, the problem of low desulfurization and degreasing rate in the existing technology is solved, efficient separation of coal and ash minerals is achieved, and the selection effect of coking coal slime is improved and Recovery rate.
Patent Information
- Application Number
- CN202410980956.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The existing technology cannot effectively carry out deep desulfurization, deaze and quality improvement of coking coal slime, resulting in a low deaze rate and is difficult to meet the needs of refined equipment.
The coking coal slime is treated with oil agglomeration treatment, the pH value of the ore slurry is adjusted, and the flocculant is added for selective flocculation, and finally reselected treatment is carried out to improve the selective separation effect between coal and ash minerals.
This method significantly improves the de-ashing rate and recovery rate of coking coal slime, and obtains fine coal with low ash content, meeting the needs of refined equipment.
Smart Images

Figure CN118892913A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coal reselection process, and in particular relates to a method for deep deashing and quality improvement of coking coal slime. Background Art
[0002] my country's coal resources can be divided into thermal coal and coking coal according to their uses, which account for 72% and 26% of my country's coal resources respectively (the other 2% is not classified clearly). Compared with my country's abundant coal resources, coking coal resources are relatively scarce.
[0003] Coal slime is a byproduct of the coal washing process. It is composed of a viscous substance consisting of fine coal particles, pulverized bone stone and water. The fine particle content in coal slime is high, and generally more than 70% of the particles are smaller than -200 mesh (0.074mm). The ash mineral composition in coal slime is mostly similar, mainly SiO2, followed by A12O3. This type of substance forms colloidal particles with strong negative charges on the surface of coal slime. The repulsion between like charges keeps these particles dispersed in water. In water, it is not only affected by gravity, but also by Brownian motion, so coal slime water often has colloidal properties. Because the charged colloid particles attract polar water molecules around it to form a "hydration film", the "hydration film" can prevent the colloid particles from contacting each other, and the coal slime water forms a stable colloidal dispersion system, which is difficult to settle naturally. Coal slime has a high moisture content and strong water retention. The moisture content of coal slime after filtration and dehydration is generally above 20%. The water content of coal slime after vacuum filtration is generally above 30%, the water content of coal slime after belt filtration is generally 26% to 40%, and the water content of coal slime after filter press filtration is generally 20% to 35%. Coal slime not only has high water content, but also has strong water retention and is not easy to dry. When naturally stored, a large amount of water in the inner layer is difficult to evaporate, making subsequent treatment more difficult. Coal slime has high ash content and low calorific value. The ash content of low-ash coal slime is generally 20% to 32%, and the calorific value is 12.5MJ / kg to 20MJ / kg; the ash content of medium-ash coal slime is 30% to 55%, and the calorific value is 8.4MJ / kg to 12.5MJ / kg; the ash content of high-ash coal slime is >55%, and the calorific value is 3.5MJ / kg to 8.4MJ / kg. Coal slime generally contains more clay minerals, and due to its high water content and fine particle size composition, most coal slimes are very viscous. It can be seen that the ash, sulfur and water content of coal sludge is relatively high, and the calorific value is low, so it is difficult to be used directly. Coal sludge is placed in open-air storage, which not only occupies a large area, but also flies all over the sky when it encounters wind and flows everywhere when it encounters water, which is very easy to cause secondary pollution, and has a great impact on the environment, ecological landscape and the safety of life and property of residents downstream of the tailings pond.
[0004] The main function of coking coal is to be used in coking production. It usually has certain adhesion and coking properties. It can coke under coking conditions in coke ovens and is used as raw coal for producing coke with certain quality requirements. The coke produced can be divided into metallurgical coke (including blast furnace coke, foundry coke and ferroalloy coke, etc.), gasification coke and calcium carbide coke, etc. The production of coking coal is directly related to industries such as metallurgy and coal chemical industry, and has an important impact on the long-term development of the national industrial system and the people's living standards. Moreover, coal is a non-renewable resource. From the perspective of the stability, harmony and sustainable development of the country and society, it is necessary to study its reasonable development and utilization scale and protect limited resources. Therefore, the by-product of coking coal washing, coal slime, is deashed and upgraded to coking raw materials, which not only has significant economic benefits, but also has obvious resource benefits. At present, the coking coal slime is mainly recycled by flotation, but the current flotation technology is mainly used for partial separation and recovery of coal slime, and its reagent system and process structure cannot meet the deep-level needs of deep desulfurization, deashing and upgrading. Coal slime flotation is a complex physical and chemical process, and the flotation effect is closely related to the properties of coal slime, reagent system, flotation process and flotation equipment. At present, the flotation technology in the coal industry is mainly used for partial separation and recovery of coal slime, and its process structure and reagent system cannot meet the deep-level needs of deep desulfurization, deashing and quality improvement. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a method for deep deashing and upgrading of coking coal slime, which aims to solve the problem that the existing deashing and upgrading methods have poor deashing rate and low recovery rate, and are difficult to meet the needs of some fine equipment such as aerospace furnaces.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A method for deep deashing and upgrading of coking coal slime, characterized by comprising the following steps:
[0008] 1) using agglomeration oil to perform oil agglomeration treatment on coking coal slime to obtain ore slurry;
[0009] 2) adjusting the pH value of the slurry obtained in step 1), then adding a flocculant, stirring and selectively flocculating to obtain a mineral solution;
[0010] 3) The ore solution obtained in step 2) is subjected to gravity separation.
[0011] In certain specific embodiments, the agglomerated oil in step 1) comprises wash oil, non-polar hydrocarbon oil and a modifier; wherein the mass ratio of the wash oil, the non-polar hydrocarbon oil and the modifier is 100:20-60:10-40;
[0012] Preferably 100:30-55:20-35;
[0013] More preferably, it is 100:40-50:20-30.
[0014] In certain specific embodiments, the non-polar hydrocarbon oil is one or more of shale oil, diesel and kerosene; and the modifier is one or more of ethyl acetate, methyl acetate and methyl formate.
[0015] In some specific embodiments, the amount of the agglomeration oil in step 1) is 1000 g / t to 10000 g / t;
[0016] Preferably 3000 g / t to 7000 g / t;
[0017] More preferably, it is 4000 g / t to 5000 g / t.
[0018] In certain specific embodiments, the oil agglomeration treatment in step 1) is specifically as follows: weighing coking coal slime, adding water and stirring to prepare slurry, then adding agglomeration oil, transferring to a ball mill for grinding, and then transferring to a stirring barrel for stirring and agglomeration to obtain ore slurry.
[0019] Furthermore, the mass concentration of coking coal slime in the slurry is 80 g / L to 350 g / L, preferably 150 g / L to 250 g / L.
[0020] In some specific embodiments, the grinding time is 1 min to 20 min, preferably 5 min to 15 min; more preferably 8 min to 10 min;
[0021] The stirring process parameters are: stirring time 5min to 15min, more preferably 8min to 10min; stirring speed 1000r / min to 2000r / min, more preferably 1400r / min to 1500r / min.
[0022] In some specific embodiments, the pH value in step 2) is 2-5; and the flocculant is one or more of organic polymer flocculants such as cationic polyacrylamide, nonionic polyacrylamide and anionic polyacrylamide; and the molecular weight of the organic polymer flocculant is 0.8×10 7 ~2×10 7 , preferably 1.2×10 7 ~1.5×10 7 .
[0023] In some specific embodiments, the amount of the flocculant used is 500 g / t to 1000 g / t;
[0024] Preferably it is 700 g / t to 800 g / t.
[0025] In certain specific embodiments, the selective flocculation in step 2) is specifically as follows: adding a buffer solution to the ore pulp after oil agglomeration, adjusting the pH to 2-5, so that the surface of the coal particles is mainly positively charged and the surface of the ash minerals is mainly negatively charged; then adding a flocculant, stirring for sufficient flocculation, and obtaining a slurry.
[0026] Furthermore, the buffer solution is a dilute sulfuric acid solution with a mass concentration of 5-15%;
[0027] Furthermore, the stirring process parameters are: stirring time is 20-50 min, more preferably 30-40 min.
[0028] In some specific embodiments, the process parameters of the gravity separation treatment in step 3) are: water flow rate is 5L / min to 15L / min, preferably 8L / min to 10L / min.
[0029] Compared with the prior art, the present invention has at least the following advantages:
[0030] The method for deep deashing and upgrading of coking coal slime provided by the present invention comprises the following steps: firstly, the coking coal slime is subjected to oil agglomeration treatment so that the hydrophobic surface of the coking coal slime is wetted, and low-specific-gravity coal particle agglomerates are formed through mutual collision between coal particles, which is beneficial to subsequent gravity separation and selective separation of ash and coal; then, the pH value of the slurry is adjusted so that the surface of the coal particles and the surface of the ash minerals have different charges, and then a flocculant is added for selective flocculation so that the ash minerals form agglomerates with high specific gravity and large particle size, which is beneficial to improving the deashing selectivity of gravity separation and obtaining clean coal with low ash content at a high recovery rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0032] Figure 1 The present invention provides a process flow chart for deep deashing and upgrading of coking coal slime. DETAILED DESCRIPTION
[0033] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0034] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0035] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0036] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0037] Embodiment 1:
[0038] The present invention provides a method for deep deashing and upgrading of coking coal slime, which comprises the following steps:
[0039] 1. Oil agglomeration of coking coal slime
[0040] Weigh coking coal slime, add water, stir and slurry to obtain slurry, control the slurry concentration to 200g / L, then add agglomeration oil, and then pour it into a ball mill for grinding for 9 minutes, pour the ground slurry into a stirring barrel, control the stirring speed to 1500r / min, stir for 10 minutes, and obtain slurry; wherein the agglomeration oil is washing oil, diesel and ethyl acetate in a weight ratio of 100:45:25, and the amount of agglomeration oil is 4500g / t.
[0041] 2. Selective flocculation
[0042] Then, a 10% dilute sulfuric acid solution was added to the slurry after oil agglomeration treatment to adjust the pH to 3, so that the surface of the coal particles was mainly positively charged and the surface of the ash minerals was mainly negatively charged; the slurry with adjusted pH value was poured into a stirring bucket and a flocculant was added and stirred for 30 minutes to obtain a modified ore liquid; wherein the flocculant was anionic polyacrylamide with a molecular weight of 1.3×10 7 , the dosage is 750g / t.
[0043] 3. Gravity separation
[0044] The ore liquid after oil agglomeration and selective flocculation is re-selected using a spiral chute; the water flow rate is 9L / min (process flow chart as follows Figure 1 As shown), gravity separation low ash clean coal, gravity separation coal and gravity separation tailings coal are obtained.
[0045] The three products obtained by gravity separation were tested for ash content. The ash content was tested by slow ashing method. According to the national standard GB / T212-2009 "Industrial Analysis Methods of Coal", a certain mass of completely dried coal slime was weighed and placed in a muffle furnace. Then, it was heated to 810±10℃ at a certain heating rate. The temperature was kept stable until the mass was constant. The mass percentage of the residue to the original mass was taken as the ash content of the sample. The specific steps and related formulas are as follows:
[0046] (1) Dry the sample. Put the filtered coal slime gravity separation product into a 100°C oven for drying. The standard for sample drying is: take the filter paper containing the sample out of the oven and place it on the laboratory bench for 3 to 4 seconds, then pick up the filter paper. If there is no watermark on the laboratory bench, it is judged that the sample has been dried;
[0047] (2) Sample preparation: Place the sample on an iron plate, grind the sample with a pressing wheel and a putty knife, and place it in a packaging bag with a corresponding label;
[0048] (3) Weighing: In an ash dish with a constant mass (mass is recorded as m1), weigh 1±0.1g of the test sample with a particle size not greater than 0.2mm, weigh it accurately to four decimal places (mass is recorded as m2), and spread it evenly in the ash dish. The mass per square centimeter should not exceed 0.15g;
[0049] (4) Place the samples, place the ash dishes into the muffle furnace in the order of weighing, close the furnace door and leave a gap of about 20 mm, raise the furnace temperature to 500°C in about 30 minutes, and maintain this temperature for 30 minutes; continue to raise the temperature to 815±10°C and maintain this temperature for 1 hour;
[0050] (5) Weighing: Close the muffle furnace, remove the ash dish from the furnace chamber, cool it in air for 5 minutes, move it into a desiccator, cool it to room temperature, and then weigh it (the mass is recorded as m3).
[0051] After the test steps are completed, the ash content of the three products is calculated according to the following formula.
[0052]
[0053] The test results of the three products prepared under the above experimental conditions according to the ash content measurement method are as follows:
[0054]
[0055] Embodiment 2:
[0056] Compared with Example 1, the only difference is that the grinding time is: Group (I): 4 min; Group (II): 15 min. The test results are:
[0057]
[0058] Embodiment 3:
[0059] Compared with Example 1, the only difference is that the mass of each substance in the agglomerated oil is: Group (I): wash oil: diesel: ethyl acetate = 100:20:10; Group (II): wash oil: diesel: ethyl acetate = 100:30:15. The test results are:
[0060]
[0061] Embodiment 4:
[0062] Compared with Example 1, the only difference is that the amount of agglomeration oil used is: Group (I): 3000 g / t; Group (II): 3500 g / t. The test results are:
[0063]
[0064] Embodiment 5:
[0065] Compared with Example 1, the only difference is that the stirring speed of the stirrer during oil agglomeration is: Group (I): 1000r / min; Group (II): 2000r / min. The test results are:
[0066]
[0067] Embodiment 6:
[0068] Compared with Example 1, the only difference is that the stirring time of the stirrer during oil agglomeration is: Group (I): 5 minutes; Group (II): 15 minutes. The test results are:
[0069]
[0070] Embodiment 7:
[0071] Compared with Example 1, the only difference is the type of flocculant added, which is: Group (I): nonionic polyacrylamide; Group (II): cationic polyacrylamide; the test results are:
[0072]
[0073] Embodiment 8:
[0074] Compared with Example 1, the only difference is the molecular weight of anionic polyacrylamide, which is: Group (I): 0.8×10 7 ; Group (II): 2×10 7 The test results are:
[0075]
[0076] Embodiment 9:
[0077] Compared with Example 1, the only difference is that the amount of anionic polyacrylamide used is: Group (I): 500g / t; Group (II): 1000g / t. The test results are:
[0078]
[0079] Embodiment 10:
[0080] Compared with Example 1, the only difference is that the water flow rate during gravity separation is different: Group (I): 5L / min; Group (II): 15L / min. The test results are:
[0081]
[0082] Embodiment 11:
[0083] Compared with Example 1, the only difference is that the mass concentration of coking coal slime in the slurry in step 1) is 100g / L, and the test results are:
[0084]
[0085] Embodiment 12:
[0086] Compared with Example 1, the only difference is that the stirring time after adding the flocculant is 20 minutes. The test results are:
[0087]
[0088] Embodiment 13:
[0089] Compared with Example 1, the only difference is that the coking coal slime is not subjected to oil agglomeration and selective flocculation, and gravity separation is directly performed after pulping. The test results are as follows:
[0090]
[0091] Embodiment 14:
[0092] Compared with Example 1, the only difference is that the coking coal slime is not subjected to selective flocculation, and is directly subjected to gravity separation after oil agglomeration. The test results are as follows:
[0093]
[0094] Embodiment 15:
[0095] Compared with Example 1, the only difference is that the coking coal slime is not subjected to oil agglomeration, and gravity separation is directly performed after selective flocculation. The test results are as follows:
[0096]
[0097] The experimental results show that compared with conventional separation methods, the clean coal obtained by this method has lower ash content and higher yield, and the separation effect of coking coal slime is improved.
[0098] In summary, from Examples 1-12, it can be seen that the selective separation effect of coal and ash minerals in the gravity separation process of coking coal slime can be improved by oil agglomeration and selective flocculation, which is conducive to obtaining low-ash and high-quality clean coal. Its selective separation effect is closely related to factors such as the composition and dosage of agglomeration oil, grinding time, agglomeration stirring speed and time, type and dosage of flocculant, gravity separation concentration and water flow rate; from Examples 13-15, it can be seen that oil agglomeration and selective flocculation operations have a certain effect on improving the gravity separation process of coking coal slime. Through the synergistic effect of oil agglomeration and selective flocculation, in the subsequent gravity separation process of coking coal slime, the yield of gravity separation clean coal can be improved and the ash content of gravity separation clean coal can be reduced.
[0099] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for deep deashing and upgrading of coking coal slime, characterized in that: The steps include: 1) using agglomeration oil to perform oil agglomeration treatment on coking coal slime to obtain ore slurry; 2) adjusting the pH value of the slurry obtained in step 1), then adding a flocculant, stirring and selectively flocculating to obtain a mineral solution; 3) The ore solution obtained in step 2) is subjected to gravity separation.
2. The method for deep deashing and upgrading of coking coal slime according to claim 1, characterized in that: The agglomerated oil in step 1) comprises washing oil, non-polar hydrocarbon oil and a modifier; wherein the mass ratio of the washing oil, the non-polar hydrocarbon oil and the modifier is 100:20-60:10-40; preferably 100:30-55:20-35; further preferably 100:40-50:20-30.
3. The method for deep deashing and upgrading of coking coal slime according to claim 2, characterized in that: The non-polar hydrocarbon oil is one or more of shale oil, diesel and kerosene; the modifier is one or more of ethyl acetate, methyl acetate and methyl formate.
4. The method for deep deashing and upgrading of coking coal slime according to claim 1, characterized in that: The amount of the agglomeration oil in step 1) is 1000 g / t to 10000 g / t, preferably 3000 g / t to 7000 g / t, and more preferably 4000 g / t to 5000 g / t.
5. The method for deep deashing and upgrading of coking coal slime according to claim 4, characterized in that: The oil agglomeration treatment in step 1) is specifically as follows: weighing coking coal slime, adding water and stirring to prepare slurry, then adding agglomeration oil, grinding, and then stirring and agglomerating to obtain ore slurry.
6. The method for deep deashing and upgrading of coking coal slime according to claim 5, characterized in that: The grinding time is 1 min to 20 min, preferably 5 min to 15 min, and more preferably 8 min to 10 min; the stirring process parameters are: stirring time 5 min to 15 min, more preferably 8 min to 10 min; stirring speed 1000 r / min to 2000 r / min, more preferably 1400 r / min to 1500 r / min.
7. The method for deep deashing and upgrading of coking coal slime according to claim 1, characterized in that: The pH value in step 2) is 2-5; the flocculant is one or more of organic polymer flocculants such as cationic polyacrylamide, nonionic polyacrylamide and anionic polyacrylamide; and the molecular weight of the organic polymer flocculant is 0.8×10 7 ~2×10 7 , preferably 1.2×10 7 ~1.5×10 7 .
8. The method for deep deashing and upgrading of coking coal slime according to claim 7, characterized in that: The usage amount of the flocculant is 500 g / t to 1000 g / t, preferably 700 g / t to 800 g / t.
9. The method for deep deashing and upgrading of coking coal slime according to claim 8, characterized in that: The selective flocculation in step 2) is specifically as follows: adding a buffer solution to the ore pulp after oil agglomeration, adjusting the pH to 2-5, and then adding a flocculant, stirring to fully flocculate, and obtaining a slurry.
10. The method for deep deashing and upgrading of coking coal slime according to claim 1, characterized in that: The process parameters of the gravity separation treatment in step 3) are: water flow rate is 5L / min to 15L / min, preferably 8L / min to 10L / min.
Citation Information
Patent Citations
Flotation of oil-agglomerated coal for ash and pyrite removal-simultaneous grinding and agglomeration
CA2172028A1
Sorting process of ultra-fine coal
CN101607225A
Hydrophobic agglomeration, sedimentation and clarification method for slime water
CN104261538A
Method for agglomerating and sorting fine coal slime by high-shearing oil
CN105750099A
Coal gasification slag separation process method
CN118002602A