Flexible actuator and preparation method thereof
By combining liquid metal, polyvinylpyrrolidone, and graphene oxide, a flexible actuator was fabricated, which solved the problem that existing flexible actuators could only respond to a single stimulus. This enabled flexible responses to multiple stimuli such as light, heat, and humidity, thus expanding the range of applications.
Patent Information
- Application Number
- CN202410941859.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flexible actuators can only respond to a single stimulus, which limits their application areas.
Flexible actuators are fabricated by combining liquid metal, polyvinylpyrrolidone, and graphene oxide. The hydrophilic functional groups and photothermal conversion capabilities of graphene oxide, along with the thermal conductivity of liquid metal, enable the actuators to respond to various stimuli such as light, heat, and humidity.
This enables flexible actuators to respond flexibly to a variety of stimuli, enhancing their application range and adaptability.
Smart Images

Figure CN118892983A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of actuators, and in particular to a flexible actuator and a preparation method thereof. Background Art
[0002] A flexible actuator is a device that can deform or move under external stimuli and has flexibility and compliance. Compared with traditional rigid actuators, flexible actuators can adapt to complex environments and changeable shapes, so they have broad application prospects in many fields. Flexible actuators can be divided into fluid actuators, chemical actuators, and electroactive polymer (EAP) actuators; however, these actuators can only respond to a single stimulus, so their application areas are limited. Therefore, how to obtain a flexible actuator that can respond to multiple stimuli has become a problem that needs to be solved urgently. Summary of the invention
[0003] The problem solved by the present invention is: how to obtain a flexible actuator with response function to multiple stimuli.
[0004] In order to solve the above problems, the present invention provides a method for preparing a flexible actuator, comprising:
[0005] Step S1, after mixing the liquid metal and polyvinyl pyrrolidone, perform a first ultrasonic dispersion treatment to obtain a first mixture;
[0006] Step S2, after mixing the first mixture with the graphene oxide dispersion liquid, performing a second ultrasonic dispersion treatment to obtain a liquid mixture;
[0007] Step S3: coating the liquid mixture on a flexible substrate and drying the mixture to form an actuating layer on the surface of the flexible substrate to obtain a flexible actuator.
[0008] Optionally, in step S2, in the liquid mixture, the mass ratio of the liquid metal, the polyvinyl pyrrolidone, and the graphene oxide is 20:20:(3-6).
[0009] Optionally, in step S3, the material of the flexible substrate is selected from one of silicone rubber and PET.
[0010] Optionally, in step S3, the thickness of the flexible substrate is 150-250 μm.
[0011] Optionally, in step S3, the thickness of the actuation layer is 100-200 μm.
[0012] Optionally, in step S1, the ultrasonic power of the first ultrasonic dispersion treatment is 50-800 W, and the time is 4-6 min.
[0013] Optionally, in step S1, the ultrasonic power of the second ultrasonic dispersion treatment is 50-800 W, and the time is 8-10 min.
[0014] Optionally, the concentration of the graphene oxide dispersion is 2-4 mg / mL.
[0015] Optionally, the liquid metal is a eutectic gallium-indium alloy.
[0016] The present invention also provides a flexible actuator, which is manufactured using the above-mentioned method for manufacturing the flexible actuator.
[0017] Compared with the prior art, the actuating layer of the flexible actuator prepared by the method of the present invention is composed of liquid metal, polyvinyl pyrrolidone and graphene oxide; wherein, polyvinyl pyrrolidone is used as a binder to enable the actuating layer to be firmly bonded to the flexible substrate; when the external humidity increases, since graphene oxide (GO) has abundant hydrophilic functional groups (such as hydroxyl and carboxyl), the hydrophilic functional groups will adsorb external water molecules, causing the actuating layer to expand rapidly, thereby driving the flexible substrate to bend; when the external humidity decreases, the shape of the flexible substrate will recover as the water molecules evaporate. When the temperature rises, the water molecules adsorbed in the actuating layer will evaporate into the external environment, causing the actuating layer to shrink, thereby driving the flexible substrate to bend; when the temperature drops to room temperature, the actuating layer gradually adsorbs water molecules in the air, and its volume will gradually recover, causing the shape of the flexible substrate to gradually recover. Under light stimulation, graphene oxide has excellent light-to-heat conversion capabilities, which converts light energy into heat energy. Liquid metal has excellent thermal conductivity, which enables heat to be quickly conducted in the actuation layer, thereby accelerating the evaporation of water molecules in the actuation layer, causing the actuation layer to shrink, thereby driving the flexible substrate to bend. When the light stimulation is removed, the temperature of the actuation layer gradually decreases, and the actuation layer gradually absorbs water molecules in the air, and its volume gradually recovers, causing the shape of the flexible substrate to gradually recover. In summary, the flexible actuator provided by the present invention has better response functions to various stimuli such as light, heat, and humidity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the process of preparing a flexible actuator in an embodiment of the present invention;
[0019] Figure 2 A physical picture of a bionic flower in an embodiment of the present invention;
[0020] Figure 3 is a graph showing the variation of deformation angle with time during the deformation process of the actuator in experimental group 1;
[0021] Figure 4is a graph showing the variation of deformation angle with time during the deformation process of the actuator in experimental group 2;
[0022] Figure 5 This is a graph showing the variation of deformation angle with time during the deformation process of the actuator in experimental group 3. DETAILED DESCRIPTION
[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0024] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0025] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0026] like Figure 1 As shown, a method for preparing a flexible actuator provided by an embodiment of the present invention includes:
[0027] Step S1, after mixing the liquid metal and polyvinyl pyrrolidone (PVP), performing a first ultrasonic dispersion treatment to obtain a first mixture;
[0028] Step S2, after mixing the first mixture with the graphene oxide dispersion liquid, performing a second ultrasonic dispersion treatment to obtain a liquid mixture;
[0029] Step S3: coating the liquid mixture on a flexible substrate and drying the mixture to form an actuating layer on the surface of the flexible substrate to obtain a flexible actuator.
[0030] The actuating layer of the flexible actuator prepared by the method of the embodiment of the present invention is composed of liquid metal, polyvinyl pyrrolidone and graphene oxide; wherein, polyvinyl pyrrolidone is used as a binder to enable the actuating layer to be firmly bonded to the flexible substrate; when the external humidity increases, since graphene oxide (GO) has abundant hydrophilic functional groups (such as hydroxyl and carboxyl groups), the hydrophilic functional groups will adsorb external water molecules, causing the actuating layer to expand rapidly, thereby driving the flexible substrate to bend; when the external humidity decreases, the shape of the flexible substrate will recover as the water molecules evaporate. When the temperature rises, the water molecules adsorbed in the actuating layer will evaporate into the external environment, causing the actuating layer to shrink, thereby driving the flexible substrate to bend; when the temperature drops to room temperature, the actuating layer gradually adsorbs water molecules in the air, and its volume will gradually recover, causing the shape of the flexible substrate to gradually recover. Under light stimulation, graphene oxide has excellent light-to-heat conversion capabilities, which converts light energy into heat energy. Liquid metal has excellent thermal conductivity, which enables heat to be quickly conducted in the actuation layer, thereby accelerating the evaporation of water molecules in the actuation layer, causing the actuation layer to shrink, thereby driving the flexible substrate to bend. When the light stimulation is removed, the temperature of the actuation layer gradually decreases, and the actuation layer gradually absorbs water molecules in the air, and its volume gradually recovers, causing the shape of the flexible substrate to gradually recover. In summary, the flexible actuator provided by the embodiment of the present invention has better response functions to various stimuli such as light, heat, and humidity.
[0031] In some embodiments of the present invention, in step S2, in the liquid mixture, the mass ratio of the liquid metal, the polyvinyl pyrrolidone, and the graphene oxide is 20:20:(3-6).
[0032] In some embodiments of the present invention, in step S3, the material of the flexible substrate is selected from one of silicone rubber and PET. Preferably, the material of the flexible substrate is PET, which has better creep resistance, better fatigue resistance and better toughness, thereby making the flexible actuator have a longer service life.
[0033] In some embodiments of the present invention, in step S3, the thickness of the flexible substrate is 150-250 μm, and the thickness of the actuation layer is 100-200 μm. The thickness of the flexible substrate is relatively thin, so that it can better respond to external stimuli and deform.
[0034] In some embodiments of the present invention, in step S1, the ultrasonic power of the first ultrasonic dispersion treatment is 50-800W and the time is 4-6min; the ultrasonic power of the second ultrasonic dispersion treatment is 50-800W and the time is 8-10min. Thus, a liquid mixture with good dispersion is obtained.
[0035] In some embodiments of the present invention, the concentration of the graphene oxide dispersion is 2-4 mg / mL.
[0036] In some embodiments of the present invention, the liquid metal is a eutectic gallium-indium alloy (EGaIn).
[0037] An embodiment of the present invention further provides a flexible actuator, which is manufactured using the method for manufacturing the flexible actuator as described above.
[0038] The embodiment of the present invention further provides a bionic flower, which is composed of four flexible actuators as described above, two square polyethylene plastic sheets and a stainless steel rod. The four flexible actuators are arranged at a 90° angle to each other, the side length of the polyethylene plastic sheet is equal to the width of the flexible actuator, and the stainless steel rod is fixed in the center. The two polyethylene plastic sheets are used to fix the four actuating films, and the fixing method can be double-sided tape. The four flexible actuators are cut into petal shapes, which can be closed under near infrared light (NIR) excitation and open under humidity stimulation. Figure 2 A physical picture of the bionic flower provided in an embodiment of the present invention.
[0039] The present invention is further described below in conjunction with specific embodiments.
[0040] Example 1
[0041] A1. After mixing 5 g of liquid metal with 5 g of polyvinyl pyrrolidone (PVP), perform a first ultrasonic dispersion treatment to obtain a first mixture; wherein the ultrasonic power of the first ultrasonic dispersion treatment is 800 W, the time is 5 min, and the liquid metal is a eutectic gallium-indium alloy.
[0042] A2. After mixing the first mixture with the graphene oxide dispersion, performing a second ultrasonic dispersion treatment to obtain a liquid mixture; wherein the concentration of the graphene oxide dispersion is 3 mg / mL, the volume is 50 mL, and the ultrasonic power of the second ultrasonic dispersion treatment is 800 W, and the time is 8 min.
[0043] A3. Coating the liquid mixture on a flexible substrate and drying it to form an actuating layer on the surface of the flexible substrate to obtain a flexible actuator; wherein the material of the flexible substrate is silicone rubber with a thickness of 200 μm, and the thickness of the actuating layer is 100 μm.
[0044] Example 2
[0045] The difference from Example 1 is that in step A3, the thickness of the actuation layer is 150 μm.
[0046] Example 3
[0047] The difference from Example 1 is that in step A3, the thickness of the actuation layer is 200 μm.
[0048] Example 4
[0049] The difference from Example 1 is that in step A3, the material of the flexible substrate is PET.
[0050] Example 5
[0051] The difference from Example 1 is that in step A2, the concentration of the graphene oxide dispersion is 3 mg / mL and the volume is 60 mL.
[0052] Example 6
[0053] The difference from Example 1 is that in step A2, the concentration of the graphene oxide dispersion is 3 mg / mL and the volume is 75 mL.
[0054] Example 7
[0055] The difference from Example 1 is that in step A2, the concentration of the graphene oxide dispersion is 3 mg / mL and the volume is 85 mL.
[0056] Experimental example, near-infrared light irradiation and humidity stimulation experiment.
[0057] Experimental Group 1
[0058] The flexible actuator prepared in Example 1 was irradiated with near-infrared light to bend the flexible substrate 180 degrees, and then the humidity of the environment was increased from 40% to 90% to restore the flexible substrate to its initial state; wherein the power of the near-infrared light was 100 W and the wavelength was 1200 nm.
[0059] Experimental Group 2
[0060] The flexible actuator prepared in Example 2 was irradiated with near-infrared light to bend the flexible substrate 180 degrees, and then the humidity of the environment was increased from 40% to 90% to restore the flexible substrate to its initial state; wherein the power of the near-infrared light was 100 W and the wavelength was 1200 nm.
[0061] Experimental Group 3
[0062] The flexible actuator prepared in Example 3 was irradiated with near-infrared light to bend the flexible substrate 180 degrees, and then the humidity of the environment was increased from 40% to 90% to restore the flexible substrate to its initial state; wherein the power of the near-infrared light was 100 W and the wavelength was 1200 nm.
[0063] The variation of deformation angle with time during the deformation of the actuator in experimental groups 1-3 is shown in Figure 3-5 ,from Figure 3-5 It can be seen that the actuators in experimental groups 1-3 can be bent 180 degrees in a short time under near-infrared light irradiation. When the humidity of the environment increases from 40% to 90%, the actuators in experimental groups 1-3 can also return to their initial state relatively quickly. It should be noted that Figure 3-5 The vertical axis is the bending angle, and the horizontal axis is time. The bending angle increases with time during the near-infrared light irradiation stage, and the bending angle decreases with time during the humidity stimulation stage.
[0064] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a flexible actuator, It is characterized in that include: Step S1, after mixing the liquid metal and polyvinyl pyrrolidone, perform a first ultrasonic dispersion treatment to obtain a first mixture; Step S2, after mixing the first mixture with the graphene oxide dispersion liquid, performing a second ultrasonic dispersion treatment to obtain a liquid mixture; Step S3: coating the liquid mixture on a flexible substrate and drying the mixture to form an actuating layer on the surface of the flexible substrate to obtain a flexible actuator.
2. The method for preparing the flexible actuator according to claim 1, It is characterized in that In the step S2, in the liquid mixture, the mass ratio of the liquid metal, the polyvinyl pyrrolidone, and the graphene oxide is 20:20:(3-6).
3. The method for preparing the flexible actuator according to claim 1, It is characterized in that In the step S3, the material of the flexible substrate is selected from one of silicone rubber and PET.
4. The method for preparing the flexible actuator according to claim 1, It is characterized in that In the step S3, the thickness of the flexible substrate is 150-250 μm.
5. The method for preparing the flexible actuator according to claim 1, It is characterized in that In the step S3, the thickness of the actuation layer is 100-200 μm.
6. The method for preparing the flexible actuator according to claim 1, It is characterized in that In the step S1, the ultrasonic power of the first ultrasonic dispersion treatment is 50-800W, and the time is 4-6 minutes.
7. The method for preparing the flexible actuator according to claim 1, It is characterized in that In the step S1, the ultrasonic power of the second ultrasonic dispersion treatment is 50-800W, and the time is 8-10 minutes.
8. The method for preparing the flexible actuator according to claim 1, It is characterized in that The concentration of the graphene oxide dispersion is 2-4 mg / mL.
9. The method for preparing the flexible actuator according to claim 1, It is characterized in that The liquid metal is a eutectic gallium-indium alloy.
10. A flexible actuator, It is characterized in that The flexible actuator is manufactured by the method for manufacturing the flexible actuator according to any one of claims 1 to 9.
Citation Information
Patent Citations
Flexible film actuator driven by sunlight
CN111224579A
MXene-based composite material as well as preparation method and application thereof
CN113968992A
Stimulation response actuator and preparation method and application thereof
CN114856949A
Photo-thermal actuating film as well as preparation method and application thereof
CN115403807A
Multi-stimulus-response soft thermal driver and preparation method thereof
CN115850833A