Method for improving surface quality of titanium alloy seamless tube

By adding Cu elements to the titanium alloy and using specific forging and lubricants, the problem of surface defects during hot extrusion of titanium alloy seamless pipes is solved, the surface quality and mechanical properties are improved, and the efficient titanium alloy seamlessness is achieved Tube preparation.

CN118893101AActive Publication Date: 2024-11-05PANZHIHUA IRON AND STEEL +1

Patent Information

Application Number
CN202411151765.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-05
Estimated Expiration
2044-08-21
Patent Text Reader

Abstract

The invention discloses a method for improving the surface quality of a titanium alloy seamless tube, which comprises the following steps: optimizing the titanium alloy component, adding 3-7% of transition element Cu, improving the plasticity of the titanium alloy, obtaining a titanium alloy bar with a uniform organization structure by adopting a reversing upsetting and diagonal upsetting switching mode, machining the bar to obtain a seamless tube rough blank, and carrying out heat treatment on the seamless tube rough blank to obtain the surface quality of the titanium alloy seamless tube. By adopting the novel glass lubricant, the fluidity of metal on the surface of the titanium alloy in the extrusion process is greatly improved, higher surface quality is obtained, and the novel glass lubricant comprises the following main chemical components: 30%-40% of SiO2, 20%-25% of NaAlO2, 7%-9% of CaTiO3, 7%-9% of B2O3, 10%-15% of NaCl and 8%-12% of MgSiO3. Through the comprehensive preparation method, the surface quality of the titanium alloy seamless tube is improved, and the mechanical property of the seamless tube is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy processing, and particularly relates to a method for improving the surface quality of a titanium alloy seamless pipe. Background Art

[0002] Titanium alloy seamless pipes have excellent mechanical properties and corrosion resistance. In recent years, they have been widely used in aerospace, ship power systems, seawater desalination and other heat exchangers, ships, offshore oil platforms and other water and oil pipelines, as well as island and reef municipal engineering pipelines. The existing preparation processes of titanium alloy seamless pipes mainly include extrusion process and oblique rolling piercing-rolling process. Compared with the oblique rolling piercing process, the extrusion method was used the earliest and most mature in my country, and extrusion forming can produce profiles with various forms and complex cross-sections, which has a status that cannot be replaced by other forming and processing technologies. However, during the extrusion process, due to the large friction coefficient and poor fluidity of titanium alloy itself, if the lubricant lubrication effect is not good during hot extrusion, it is easier to adhere to the extrusion die material, and it is easy to form defects such as longitudinal scraping lines, pockmarks, bubbles, peeling, flash, and burrs on the surface of the profile. Commonly used lubricants are grease, glass lubricant and metal coating. Among them, glass lubricant is the lubricating material with the most development potential, but a suitable glass lubricant has not yet been found to achieve industrial application level. Summary of the invention

[0003] In order to solve the bottleneck problem existing in the above-mentioned prior art, the present invention changes the composition of titanium alloy to improve its own plasticity. On this basis, a new lubricant is used to improve the hot extrusion lubrication effect, so that the prepared seamless pipe has excellent mechanical properties and the surface quality of the seamless pipe is significantly improved. It can be applied to important or key components such as hydraulic pipelines and fuel pipelines of aircraft.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides a method for improving the surface quality of a titanium alloy seamless tube, the method comprising the following steps:

[0005] ① Add transition element Cu to raw materials (such as first-grade and above titanium sponge, aluminum alloy or aluminum beans and aluminum foil, and corresponding grade metal stabilizing elements), with a mass content of Cu element of 3% to 7%, mix and press into multiple electrode blocks, and obtain consumable electrodes after welding multiple electrode blocks. Adding transition element Cu is mainly used to improve the plasticity of the alloy.

[0006] ② The consumable electrode obtained in step ① is smelted 2 to 3 times in a vacuum consumable arc furnace to obtain a titanium alloy ingot.

[0007] ③ The titanium alloy ingot obtained in step ② is kept at 880℃~1100℃ for 4~5h, and then subjected to 6 fires of upsetting and rolling to form titanium alloy bars. The upsetting adopts the switching mode of xyz reversing upsetting and diagonal reversing upsetting; xyz reversing upsetting adopts three-pier and three-drawing, and diagonal reversing upsetting adopts four-pier and four-drawing, and the deformation of each fire is 40%~50%; after the first fire of xyz reversing upsetting, the second fire is diagonal reversing upsetting, and so on, that is, after each xyz reversing upsetting, it is replaced with diagonal reversing upsetting, and the two upsetting modes are operated alternately, and the last fire is drawn and rolled into bars. This forging method can significantly improve the uniformity of the forged bar structure, reduce the segregation of Cu elements, and improve the subsequent extrusion pass rate and surface quality.

[0008] ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, and the fine forged bar is annealed at an annealing temperature of [T-(120-200)]°C for 1-2 hours, wherein T is the phase transition point temperature in °C. After annealing and straightening, the bar is subjected to polishing and drilling to obtain a titanium alloy seamless pipe rough blank.

[0009] ⑤Heat the titanium alloy seamless tube rough blank obtained in step ④ to a heating temperature of [T-(50-80)]°C, wherein T is the phase transition point temperature in °C. Then add a small amount of water to the new glass lubricant and apply it on the inner and outer surfaces of the tube blank. The main chemical components of the new glass lubricant include SiO2: 30%-40%, NaAlO2: 20%-25%, CaTiO3: 7%-9%, B2O3: 7%-9%, NaCl: 10%-15% and MgSiO3: 8%-12%. The addition of magnesium metasilicate is beneficial to reducing the friction coefficient of the lubricant.

[0010] ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder, and the obtained seamless tube is vacuum annealed and pickled, and the annealing temperature is [T-(150-400)]°C, and the holding time is 1-2h. Wherein, T is the phase transition point temperature, in °C.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] The present invention optimizes the composition of titanium alloy, improves the plasticity of titanium alloy, adopts the switching mode of reversing upsetting and diagonal upsetting to obtain titanium alloy rods with uniform organizational structure, obtains seamless tube rough blanks after machining the rods, and adopts new glass lubricants to greatly improve the fluidity of the metal on the surface of titanium alloy during the extrusion process, thereby obtaining higher surface quality. Through the above comprehensive preparation method, not only the surface quality of titanium alloy seamless tubes is improved, but also the mechanical properties of seamless tubes are greatly improved. DETAILED DESCRIPTION

[0013] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.

[0014] Example 1

[0015] A method for improving the surface quality of titanium alloy seamless pipes, producing TA18 titanium alloy seamless pipes with specifications of Φ48×12mm, the specific process flow is:

[0016] ① The raw materials are mixed to press a plurality of electrode blocks, the plurality of electrode blocks are welded to obtain a consumable electrode, and a transition element Cu is added; the mass content of the Cu element is 3%.

[0017] ② The consumable electrode obtained in step ① is smelted twice in a vacuum consumable arc furnace to obtain a titanium alloy ingot; the ingot specification is Φ550mm.

[0018] ③ The titanium alloy ingot obtained in step ② is kept at 880°C for 5h, and subjected to 6 fires of upsetting and rounding to form a titanium alloy bar (machining). The upsetting and drawing adopts the switching mode of xyz reversing upsetting and diagonal reversing upsetting and drawing; odd-numbered fires of reversing upsetting and drawing (three upsetting and three drawing) → even-numbered fires of diagonal upsetting and drawing (four upsetting and four drawing), and the last fire (sixth fire) is upsetting and forging (drawing and lengthening and rounding).

[0019] ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, and the fine forged bar (Φ150mm bar) is annealed (750℃ / 2h), and after annealing and straightening, it is polished and drilled to Φ130*Φ30mm to obtain a titanium alloy seamless pipe rough blank.

[0020] ⑤ Heat the titanium alloy seamless tube rough billet obtained in step ④ to 900°C; then apply glass lubricant on the inner and outer surfaces of the tube billet; the main chemical components of the new glass lubricant include SiO2: 38%, NaAlO2: 22%, CaTiO3: 8%, B2O3: 8%, NaCl: 13% and MgSiO3: 11%.

[0021] ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder to obtain a Φ48×12mm seamless tube, which is then vacuum annealed and pickled; the annealing temperature is 700°C and the holding time is 2h.

[0022] The TA18 titanium alloy seamless tube prepared in Example 1 has a smooth outer surface without any defects such as grooves, scratches and abrasions, a tensile strength of 800 kPa, and an elongation of 24%.

[0023] Example 2

[0024] A method for improving the surface quality of titanium alloy seamless pipes, producing TA18 titanium alloy seamless pipes with specifications of Φ48×12mm, the specific process flow is:

[0025] ① The raw materials are mixed to press a plurality of electrode blocks, the plurality of electrode blocks are welded to obtain a consumable electrode, and a transition element Cu is added; the mass content of the Cu element is 7%.

[0026] ② The consumable electrode obtained in step ① is smelted three times in a vacuum consumable arc furnace to obtain a titanium alloy ingot; the ingot specification is Φ550mm.

[0027] ③ The titanium alloy ingot obtained in step ② is kept at 1100℃ for 4h, and subjected to 6 fires of upsetting and rolling into titanium alloy bars (machining). The upsetting and drawing adopts the switching mode of xyz reversing upsetting and diagonal reversing upsetting and drawing; odd-numbered fires of reversing upsetting and drawing (three upsetting and three drawing) → even-numbered fires of diagonal upsetting and drawing (four upsetting and four drawing), and the last fire (sixth fire) is upsetting and forging (drawing and lengthening and rolling).

[0028] ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, and the fine forged bar (Φ150mm bar) is annealed (750℃ / 2h), and after annealing and straightening, it is polished and drilled to Φ130*Φ30mm to obtain a titanium alloy seamless pipe rough blank.

[0029] ⑤ Heat the titanium alloy seamless tube rough blank obtained in step ④ to 900°C, wherein T is the phase transition point temperature; then apply glass lubricant on the inner and outer surfaces of the tube blank; the main chemical components of the new glass lubricant include SiO2: 38%, NaAlO2: 25%, CaTiO3: 7%, B2O3: 8%, NaCl: 12% and MgSiO3: 10%.

[0030] ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder to obtain a Φ48×12mm seamless tube, which is then vacuum annealed and pickled; the annealing temperature is 700°C and the holding time is 2h.

[0031] The TA18 titanium alloy seamless tube prepared in Example 2 has a smooth outer surface without any defects such as grooves, scratches and abrasions, a tensile strength of 780 kPa, and an elongation of 26%.

[0032] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for improving the surface quality of a titanium alloy seamless pipe, characterized in that: The method comprises the following steps: ① The raw materials are mixed and pressed into multiple electrode blocks, and the multiple electrode blocks are welded to obtain consumable electrodes, and the transition element Cu is added; ② The consumable electrode obtained in step ① is melted 2 to 3 times in a vacuum consumable arc furnace to obtain a titanium alloy ingot; ③ The titanium alloy ingot obtained in step ② is kept at 880° C. to 1100° C. for 4 to 5 hours, and subjected to 6 rounds of upsetting and rolling to form a titanium alloy bar, wherein the upsetting adopts a switching mode of xyz reversing upsetting and diagonal reversing upsetting; ④ The bar obtained in step ③ is subjected to no less than two rounds of fine forging, the fine forged bar is annealed, and after annealing and straightening, it is subjected to lathing and drilling to obtain a titanium alloy seamless pipe rough blank; ⑤ heating the titanium alloy seamless tube blank obtained in step ④ to a temperature of T-(50-80)°C, where T is the phase transition point temperature; and then applying a glass lubricant to the inner and outer surfaces of the tube blank; ⑥ The lubricated seamless tube obtained in step ⑤ is extruded by a horizontal extruder, and the obtained seamless tube is vacuum annealed and pickled; the annealing temperature is T-(350-500)°C, and the holding time is 1-2h.

2. The method according to claim 1, characterized in that In step ①, the mass content of the Cu element is 3% to 7%.

3. The method according to claim 2, characterized in that In step ③, the xyz reversing upsetting and drawing adopts three upsetting and three drawing, and the diagonal reversing upsetting and drawing adopts four upsetting and four drawing, and the deformation amount of each fire is 40% to 50%.

4. The method according to claim 3, characterized in that Step ③ The two upsetting modes are operated alternately, and each time the xyz reversing upsetting is replaced by the diagonal reversing upsetting.

5. The method according to claim 4, characterized in that In step ④, the annealing temperature is T-(120-200)°C, and the holding time is 1-2h, wherein T is the phase transition point temperature.

6. The method according to claim 5, characterized in that Step ⑤: The main chemical components of the glass lubricant include SiO2: 30% to 40%, NaAlO2: 20% to 25%, CaTiO3: 7% to 9%, B2O3: 7% to 9%, NaCl: 10% to 15% and MgSiO3: 8% to 12%.

Citation Information

Patent Citations

  • Preparation method of titanium alloy seamless pipe

    CN112439806A

  • Method for increasing shrinkage strain ratio of TA18 titanium alloy seamless tube and TA18 titanium alloy seamless tube

    CN116656994A

  • Weak-texture TA18 titanium alloy bar and preparation method thereof

    CN116770116A

  • Titanium alloy seamless tube and preparation method thereof

    CN117358778A

  • Smelting and forging method for titanium alloy with low component range

    CN117551904A

Cited By

  • Method for improving yield of TA18 titanium alloy seamless tube

    CN119972849A