Friction brazing method for CGA device packaging
By forming a low melting point coating on the copper column surface of CGA devices and adopting friction brazing technology, the problems of high mold assisted positioning cost in traditional processes and low adhesion in mold-free assisted processes are solved, and the high strength of the solder joints is achieved and high-quality connection.
Patent Information
- Application Number
- CN202411097933.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-05
AI Technical Summary
In the packaging process of CGA devices, traditional methods have problems such as high precision mold assisted positioning cost, poor wetting of solder joints and high porosity; in the mold-free auxiliary method, the interface connection layer is polished and thinned and has low adhesion; the improvement method In the meantime, the dip tin coating is insufficiently diffused, resulting in limited solder joint strength.
The low-melting point coating material is used to form a continuous intermetallic compound layer on the surface of the copper column, and through friction brazing technology, the friction between the low-melting point coating and the brazing ball generates a heat-machine effect to form a reliable friction brazing connection. Improve the strength and quality of solder joints.
Improve the connection strength of solder joints, solve the cost and quality problems in mold-assisted processes, enhance the adhesion in mold-free auxiliary processes, overcome the problem of insufficient diffusion of dipped tin coating, and significantly improve the CGA devices Package quality.
Smart Images

Figure CN118893261A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microelectronic packaging and microconnection, and in particular to a friction brazing method for CGA device packaging. Background Art
[0002] In the field of microelectronic packaging, the ball grid array (BGA) packaging form is widely used because its input / output pins are arranged on the bottom surface of the chip carrier substrate and arranged in an array rather than around the device. Therefore, it has the advantages of a large number of input / output pins and a larger pin spacing under the same number of pins. However, due to the large difference in thermal expansion coefficients between the chip carrier substrate and the printed circuit board, the interior of the array solder balls between the two is very likely to produce large cyclic thermal stress due to the power cycle load during the service of the device, so the reliability and service life of the BGA packaged device are not high. To address this problem, the column grid array (CGA) packaging form was developed to improve the reliability and life of the surface array packaged device. The CGA package replaces the array-arranged solder balls of the BGA package with array-arranged solder columns, and uses the flexural deformation of the flexible copper columns with a larger aspect ratio to release the thermal stress under the power cycle load. Therefore, the reliability and life of the CGA device are significantly improved and widely used in aerospace, communications, military industry, automotive electronics and other fields. However, the copper pillar has a large aspect ratio and poor stability, and its welding difficulty is much greater than that of BGA solder balls. At present, the packaging of CGA devices usually uses precision molds to position the copper pillars, and then uses the reflow soldering method for connection. However, in addition to the problems of poor versatility and high cost of precision molds, the presence of molds during the welding process also affects the effective transfer of heat from the heat source and the volatilization of flux gas in the solder paste, which easily produces poor wetting and high porosity solder joints. In addition, the tiny solder pillars are easily scratched during the disassembly of the mold after welding.
[0003] The currently developed CGA copper column connection method that does not require mold-assisted positioning is to use a micro-precision drilling machine to clamp the copper column and align it with the solder ball on the pad arranged in an array on the substrate, so that the copper column rotates at a specific speed and is pressed down at a specific axial feed speed to drill into the predetermined depth inside the solder ball, and the connection of the copper column is realized by the frictional heat-mechanical effect between the copper column and the solder ball during the feed. This copper column connection method without mold assistance does not require a set of high-precision molds to be customized for each specification of CGA device, so the cost is greatly reduced, and the problems of poor wetting and high porosity caused by the presence of precision molds during welding are avoided. This connection method also has the advantages of low process temperature, simple welding equipment, easy automation, and suitable for the production of CGA devices of various specifications. However, with the deepening of research, it is found that the copper column connection method without mold assistance still has the following problems:
[0004] (1) The interface connection layer formed during welding is easily thinned while growing due to the grinding effect of the brazing filler metal in the subsequent stage, and may even be completely ground away in the local interface area with high stress, which limits the improvement of the connection strength of the solder joint;
[0005] (2) The formed interface connection layer no longer presents a scallop shape with mechanical interlocking effect, and the improvement of the connection strength of the solder joint is limited by this.
[0006] (3) The thermal physical and mechanical properties of copper and solder are very different, resulting in a large difference in the thermal physical state between the two during welding, resulting in weak adhesion between the copper column and the solder ball, and easy cracking of the interface above the solder joint during cooling.
[0007] (4) In the improved method developed to address the above problem, the copper column is tinned before welding, and then the copper column is subjected to rotational friction embedded welding. Although the connection strength is improved, the melting point of the tinned coating and the solder ball is higher than the peak temperature of the friction pair interface, and the embedded friction welding remains in the solid phase welding nature. As a result, the traces of the tinned coating / solder friction pair interface in the upper area of the copper column side after welding are very obvious and there are micro-areas that have not achieved substantial connection, which means that the adhesion in the upper area of the copper column side is not strong and the mutual diffusion is not sufficient. Therefore, the improvement of the connection strength of the solder joint is also limited by this. Summary of the invention
[0008] The present invention aims to solve the problems of high cost, poor solder joint wetting and high porosity caused by the need for precision mold-assisted positioning of copper pillars in the traditional CGA packaging process; the present invention aims to solve the problem that the connection quality of copper pillars in the developed mold-free CGA packaging process is limited by the low adhesion between the copper pillars and the solder with different performances due to the continuous grinding and thinning of the interface connection layer during the connection, and the limited improvement of the connection strength; the present invention aims to solve the problem that the interface diffusion of the tin-immersion coating / solder friction pair in the upper area of the copper pillar side surface is insufficient, the interface marks in the interface area are very obvious, and the local micro-area does not achieve substantial connection, resulting in limited improvement of the solder joint connection strength.
[0009] The present invention is achieved through the following technical methods:
[0010] A friction brazing method for CGA device packaging comprises the following steps:
[0011] Step 1: Preparation of low melting point coating on the surface of copper column:
[0012] According to the designed ratio of various alloy elements, the low melting point coating material is prepared and the vacuum degree is 3×10 -3The alloy is melted in a vacuum high-frequency induction melting device of Pa to form a low-melting-point coating material with uniform composition; the low-melting-point coating material is then heated and melted in a quartz crucible, and a low-melting-point coating is formed on the surface of a copper column of a standard size within a specific length range at one end thereof by a hot dip method;
[0013] Step 2: performing low-temperature aging treatment on the copper pillar with the low-melting-point coating formed on the surface, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the copper pillar / low-melting-point coating;
[0014] Step 3: Print an appropriate amount of solder paste on the pads arranged in the array;
[0015] Step 4, heating the solder paste to wet the array-arranged pads, and forming a spherical crown-shaped solder ball array with uniform shape and size on the array-arranged pads;
[0016] Step 5: Welding of copper pillars with low melting point coating on a single surface:
[0017] Ultrasonic cleaning is used to remove impurities and oxides on the surface of the copper column with a low melting point coating formed on the surface; the copper column with a low melting point coating formed on the surface is clamped in the drill chuck of a micro-precision drilling machine, and the movement of the substrate where the pad is located is controlled by a program so that the copper column with a low melting point coating formed on the surface is located above the pad and is aligned with the center of the solder ball on the pad; the drill chuck of the micro-precision drilling machine is used to drive the copper column with a low melting point coating formed on the surface to rotate at a rotation speed of n1 and press down, and after the end of one end of the copper column with a low melting point coating formed on the surface is in close contact with the top of the solder ball, The axial feeding of the copper column with a low melting point coating on the surface is stopped and its original rotation speed is maintained to preheat the contact surface between the two; after preheating for t1 time, the copper column with a low melting point coating on the surface is controlled to be axially pressed downward at a uniform feeding speed v1 and drilled into a predetermined depth S inside the solder ball; the axial feeding of the copper column with a low melting point coating on the surface is stopped and it is rotated at the original rotation speed for t2 time to perform heat preservation treatment on the solder joint; then the copper column with a low melting point coating on the surface is kept still to cool the solder joint for t3 time; the drill chuck is opened and lifted and the surface is formed The copper pillar with low melting point coating remains in the spherical crown solder ball on the pad, completing the welding of the copper pillar with low melting point coating on a single surface; during welding, the adhesion friction heat generation and interface temperature of the friction pair between the low melting point solder coating and the solder ball with similar performance are both high, and the low melting point coating at the interface of the friction pair is transformed into a thermoplastic state and then melted; the liquid low melting point coating solder flows, fills and wets the "barrel-shaped" friction pair interface of the solder ball under the action of axial, tangential and radial extrusion stresses during welding, and forms Reliable friction brazing connection; Due to the heat-mechanical effect, the low-melting-point coating and solder on both sides of the friction interface also undergo atomic mutual diffusion, adhesion, and dynamic recrystallization during welding. In the early stage of welding, there are plastic deformation connection mechanisms, diffusion connection mechanisms, and recrystallization connection mechanisms between solid phase materials, which are transformed into dissolution-diffusion connection mechanisms of brazing between liquid and solid phases in the later stage of welding; After welding, no traces of the interface of the low-melting-point coating / solder friction pair and areas where no substantial connection is achieved are observed in the bottom, middle, and upper areas of the bottom and side surfaces of the copper column of the solder joint;
[0018] Step 6: Welding of copper pillar array with low melting point coating on the surface:
[0019] Repeat the process of step 5 above with the same size parameters and process parameters, and weld the copper pillars with low-melting-point coating on the surface of each array-arranged pad one by one, and ensure that the exposed end height of the copper pillar array with low-melting-point coating on the surface after welding is consistent.
[0020] Preferably, the copper column described in step 1 is any one of a pure copper column, a brass column, a tin bronze column, and a beryllium copper column of uniform specifications and sizes prepared according to standards; the aspect ratio of the copper column ranges from 5 to 20, and the diameter d of the copper column is not less than 1 / 4 of the pad diameter D and not more than 2 / 5 of the pad diameter D.
[0021] Preferably, the low melting point coating material described in step 1 is any one of BiInSn, BiPbSn, PbInSn, SnBiInZn, SnPbInBiSb, SnIn, and SnBi solders; the process for preparing the low melting point coating material described in step 1 is to first heat it to 40 to 60°C above the melting point (or liquidus) of the metal with the highest melting point in the coating material components for melting, and then gradually reduce the heating temperature to 40 to 60°C above the eutectic point (or liquidus) of the coating material for melting, and the melting time is 10 to 40 minutes.
[0022] Preferably, the process temperature of the hot dipping in step 1 is 35°C to 60°C above the eutectic point (or liquidus) temperature of the coating material, the hot dipping time is 30 to 120 seconds, and the thickness of the low-melting-point coating formed is 10 to 50 microns.
[0023] Preferably, the hot dipping method described in step 1 forms a low melting point coating on the surface within a specific length range of one end of a copper column of standard size, the specific length range being 6d to 10d, where d is the diameter of the copper column.
[0024] Preferably, the low-temperature aging temperature range of the copper column with the low-melting-point coating formed on the surface in step 2 is 50° C. to 100° C., and the low-temperature aging time is 0.5 to 6 hours.
[0025] Preferably, after low-temperature aging of the copper pillar with the low-melting-point coating formed on the surface in step 2, the thickness of the intermetallic compound layer formed between the copper pillar / the low-melting-point coating is 1.0 to 2.5 microns.
[0026] Preferably, the array-arranged pads described in step 3 are array-arranged pads on a chip carrier substrate or array-arranged pads on a printed circuit board; the friction brazing method for CGA device packaging is suitable for connecting copper columns on array-arranged pads on a chip carrier substrate in the first-level packaging, and is also suitable for connecting copper columns on array-arranged pads on a printed circuit board in the second-level packaging.
[0027] Preferably, the type of the array-arranged pads described in step 3 is any one of a pure copper pad, a pure copper pad containing a Ni surface layer, and a pure copper pad containing an Au / Ni surface layer.
[0028] Preferably, the type of solder in the solder paste described in step 4 is any one of SnCu series, SnAg series, SnAgCu series, SnSb series, SnBiAg series, SnBiAgCu series, and SnZnBi series soft solder.
[0029] Preferably, the heating temperature of the solder paste in step 4 is 30°C to 55°C above the eutectic point (or liquidus) temperature of the solder in the solder paste, and the height h of the spherical crown solder balls formed in the array is greater than 7 / 10 of the pad diameter D.
[0030] Preferably, the copper column with a low-melting-point coating on its surface described in step 5 is clamped in the drill chuck of a micro-precision drilling machine, and the exposed end length of the copper column with a low-melting-point coating on its surface is 1.2 to 2.5 times the height h of the spherical crown solder ball.
[0031] Preferably, in step 5, the copper column with the low-melting-point coating formed on the surface is driven by the drill chuck of the micro-precision drilling machine to rotate at a rotation speed of n1, and the rotation speed n1 ranges from 5000 rpm to 12000 rpm.
[0032] Preferably, the preheating time t1 during which the end of the copper column with the low-melting-point coating formed on the surface of step 5 is in close contact with the top of the solder ball and the original rotation speed n1 is maintained is 5 seconds to 25 seconds.
[0033] Preferably, the copper column with a low-melting-point coating on the surface described in step 5 is axially pressed downward at a uniform feed speed v1 and drilled into a predetermined depth S inside the solder ball. The axial feed speed v1 ranges from 10 to 60 microns / second, and the predetermined depth S ranges from 0.6h to h-0.1mm, where h is the height of the array spherical crown-shaped solder balls.
[0034] Preferably, in step 5, the axial feeding of the copper column with the low melting point coating formed on the surface is stopped and the copper column is rotated at the original rotation speed for t2 time to perform heat preservation treatment on the solder joint, and the heat preservation time t2 ranges from 5 to 30 seconds.
[0035] Preferably, in step 5, the copper pillar with the low melting point coating formed on the surface is kept still to allow the solder joint to cool for a time t3, and the cooling time t3 is in the range of 15 to 60 seconds.
[0036] The present invention has the following beneficial effects:
[0037] First, the low-melting-point coating and low-temperature aging treatment on the surface of the copper column of the present invention form a continuous scallop-shaped intermetallic compound layer with appropriate thickness between the copper column and the low-melting-point coating. During welding, the low-melting-point coating is between the intermetallic compound layer and the solder ball, so that the intermetallic compound layer will not be ground away. Therefore, there is no problem that "the interface connection layer formed during welding is easily thinned while growing due to the grinding action of the solder in the subsequent stage, and may even be completely ground away in the local interface area with greater stress, and the improvement of the connection strength of the solder joint is limited by this."
[0038] Second, the low-melting-point coating and low-temperature aging treatment on the surface of the copper column of the present invention form a continuous scallop-shaped intermetallic compound layer with a suitable thickness between the copper column and the low-melting-point coating. During welding, the low-melting-point coating is between the intermetallic compound layer and the solder ball so that the intermetallic compound layer will not be polished. Therefore, there is no problem that "the formed interface connection layer no longer presents a scallop shape with mechanical interlocking effect, and the connection strength improvement of the solder joint is limited by this."
[0039] Third, the low-melting-point coating and low-temperature aging treatment on the surface of the copper column of the present invention form a continuous scallop-shaped intermetallic compound layer with appropriate thickness between the copper column and the low-melting-point coating. During welding, the low-melting-point coating is between the intermetallic compound layer and the solder ball, and the friction pair welding between the copper column / solder heterogeneous materials with a huge performance difference is transformed into a friction pair welding between homogeneous or similar materials between the low-melting-point solder coating / solder. The friction heat generation, interface temperature, mutual diffusion ability of atoms on both sides of the interface and adhesion of materials on both sides of the friction pair interface are improved, and there is no problem of "the thermal physical and mechanical properties of copper and solder are very different, resulting in a large difference in thermal physical state between the two during welding, resulting in weak adhesion between the copper column and the solder ball, and easy cracking of the interface above the solder joint during cooling."
[0040] Fourth, during welding, the low melting point coating of the present invention is located between the intermetallic compound layer and the solder ball, which transforms the friction pair welding between the copper column / solder heterogeneous materials with greatly different performance into the friction pair welding between the low melting point solder coating / solder homogeneous or similar materials, significantly increases the friction heat generation and interface temperature, and partially melts after the low melting point coating at the friction pair interface is transformed into a thermoplastic state; the liquid low melting point coating solder flows at the "barrel-shaped" friction pair interface under the action of axial, tangential and radial extrusion stresses during welding, fills and wets the "barrel-shaped" friction pair interface of the solder ball and forms a reliable friction brazing connection. The improved embedded friction welding method overcomes the problems of "the melting point of the tin-containing coating and the solder ball is higher than the peak temperature of the friction pair interface, the embedded friction welding remains in the solid phase welding nature, and the traces of the tin-containing coating / solder friction pair interface in the area above the side of the copper column after welding are very obvious and there are micro-areas without actual connection, which means that the adhesion in the area above the side of the copper column is not strong and the mutual diffusion is not sufficient, so the improvement of the connection strength of the solder joint is also limited by this."
[0041] Fifth, a friction brazing method for CGA device packaging of the present invention, compared with the traditional connection method of mold positioning copper pillars and reflow soldering connection used in the field of microelectronic packaging technology, can save expensive precision mold costs and overcome the problems of poor solder joint wetting and high porosity caused by the use of precision molds; compared with the existing CGA device copper pillar embedded friction welding connection method without mold auxiliary positioning, the solder joint connection strength can be increased by 64.9%; compared with the improved CGA device copper pillar embedded friction welding method without mold auxiliary positioning, the solder joint connection strength can be increased by 22.2%, and the connection quality is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic diagram of the solder joint structure after friction brazing of a pure copper column with a low-melting-point coating formed on a single surface in the first specific implementation mode;
[0043] Figure 2 This is a schematic diagram of the welding point structure of a brass column with a low-melting-point coating formed on a single surface after friction brazing in the second specific implementation mode;
[0044] Figure 3 A schematic longitudinal section of a single interconnection structure after one end of the pure copper column with a low melting point coating formed on the surface thereof in Example 1 is connected by friction brazing and then the other end of the pure copper column without coating is connected by low temperature reflow soldering;
[0045] Figure 4 This is a schematic longitudinal section of a single interconnected structure after one end of the brass column with a low melting point coating formed on the surface is connected by friction brazing and the other end of the brass column without coating is connected by low temperature reflow soldering in Example 2. DETAILED DESCRIPTION Specific implementation method one:
[0047] A friction brazing method for CGA device packaging comprises the following steps:
[0048] Step 1: Preparation of low melting point coating on the surface of pure copper column:
[0049] According to the designed ratio of various alloy elements, the low melting point coating material is prepared and the vacuum degree is 3×10 -3 The alloy is melted in a vacuum high-frequency induction melting device of Pa to form a low-melting-point coating material with uniform composition and then cooled for standby use; impurities and oxides on the surface of a pure copper column of standard size are removed by ultrasonic cleaning; the low-melting-point coating material is heated and melted in a quartz crucible, and a low-melting-point coating is formed on the surface within a specific length range of one end of the pure copper column of standard size by hot dipping; the thickness of the formed low-melting-point coating should be not less than 10 microns and not more than 50 microns, and the thickness of the low-melting-point coating should be uniform, the surface should be bright, and there should be no balling or weak wetting phenomenon;
[0050] Step 2: performing low-temperature aging treatment on the pure copper column with the low-melting-point coating formed on the surface, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the pure copper column / low-melting-point coating;
[0051] Step 3, printing an appropriate amount of solder paste on the array-arranged pads of the printed circuit board;
[0052] Similar to the traditional BGA ball planting process, a proper amount of solder paste is printed on the array-arranged pads of the printed circuit board using a template printing process, and the amount of solder paste printed on the array-arranged pads is required to be consistent;
[0053] Step 4, heating the solder paste to wet the array-arranged pads of the printed circuit board, and forming a spherical crown-shaped solder ball array with uniform shape and size on the array-arranged pads;
[0054] During the heating process, the flux in the solder paste is first activated and removes the oxide film on the surface of the pad through chemical reaction, and then the solder in the solder paste melts, wets the array-arranged pads, and forms a spherical crown-shaped solder ball array with a consistent height on the array-arranged pads of the printed circuit board under the action of surface tension;
[0055] Step 5: Welding of a pure copper column with a low melting point coating formed on a single surface:
[0056] Ultrasonic cleaning is used to remove impurities and oxides on the surface of the pure copper column with a low melting point coating formed on the surface; the pure copper column with a low melting point coating formed on the surface is clamped in the drill chuck of a micro-precision drilling machine, and the movement of the printed circuit board where the pad is located is controlled by a program so that the pure copper column with a low melting point coating formed on the surface is located above the pad and is aligned with the center of the solder ball on the pad; the pure copper column with a low melting point coating formed on the surface is driven by the drill chuck of the micro-precision drilling machine to rotate and press down at a rotation speed of n1, and the surface is stopped after the end of one end of the pure copper column with a low melting point coating formed on the surface is in close contact with the top of the solder ball. The pure copper column with a low melting point coating on its surface is axially fed and maintained at its original rotation speed to preheat the contact surface between the two; after preheating for t1 time, the pure copper column with a low melting point coating on its surface is controlled to be axially pressed down at a uniform speed of v1 and drilled into a predetermined depth S inside the solder ball; the axial feeding of the pure copper column with a low melting point coating on its surface is stopped and the column is rotated at the original rotation speed for t2 time to perform heat preservation treatment on the solder joint; then the pure copper column with a low melting point coating on its surface is kept still to cool the solder joint for t3 time; the drill chuck is opened and lifted and the pure copper column with a low melting point coating on its surface is left In the spherical crown solder ball on the pad, the welding of a single pure copper column with a low-melting-point coating on the surface is completed; during welding, the adhesion friction heat generation and interface temperature of the friction pair between the low-melting-point solder coating and the solder ball with similar performance are both high, and the low-melting-point coating at the interface of the friction pair is transformed into a thermoplastic state and then melted; under the action of axial, tangential and radial extrusion stresses during welding, the liquid low-melting-point coating solder flows, fills and wets the "barrel-shaped" friction pair interface of the solder ball and forms a reliable friction brazing connection; the low-melting-point coating on both sides of the friction interface Due to the thermal-mechanical effects, the point coating and solder undergo atomic mutual diffusion, adhesion, and dynamic recrystallization during welding. In the early stage of welding, there are plastic deformation connection mechanisms, diffusion connection mechanisms, and recrystallization connection mechanisms between solid phase materials, which are transformed into dissolution-diffusion connection mechanisms of brazing between liquid and solid phases in the later stage of welding. Compared with the improved embedded friction welding method of copper pillars of CGA devices without mold-assisted positioning, no traces of the interface of the low-melting-point coating / solder friction pair and no areas where substantial connection is achieved are observed in the lower, middle, and upper areas of the bottom and side surfaces of the pure copper pillars of the solder joints after welding.
[0057] The schematic diagram of the solder joint structure after friction brazing of a pure copper column with a low melting point coating on a single surface is shown in Figure 1 As shown, 1 is a printed circuit board; 2 is a solder pad on the printed circuit board; 3 is a solder resist film on the printed circuit board; 4 is a cylindrical pure copper column of standard size; 5 is a low-melting-point coating on the surface of the pure copper column; 6 is an intermetallic compound layer generated between the pure copper column and the low-melting-point coating; 7 is a spherical crown-shaped solder ball formed by the solder paste on the solder pad after reflow soldering; 8 is a crystallized area formed after the low-melting-point coating undergoes the melting and cooling solidification process during soldering.
[0058] Step 6: Connection of pure copper column array with low melting point coating formed on the surface:
[0059] Repeat the process of step 5 above with the same size parameters and process parameters, and weld the pure copper pillars with a low-melting-point coating on the surface of each array-arranged pad on the printed circuit board one by one, and ensure that the exposed end height of the pure copper pillar array with a low-melting-point coating on the surface is consistent after welding.
[0060] The present invention can be used to achieve high-quality connection of surface array packaging devices with high frequency, high power and high reliability requirements in the fields of aerospace, communications, military industry, automotive electronics, etc. Specific implementation method 2:
[0062] A friction brazing method for CGA device packaging comprises the following steps:
[0063] Step 1: Preparation of low melting point coating on the surface of brass column:
[0064] According to the designed ratio of various alloy elements, the low melting point coating material is prepared and the vacuum degree is 3×10 -3 The alloy is melted in a vacuum high-frequency induction melting device of Pa to form a low-melting-point coating material with uniform composition and then cooled for use; impurities and oxides on the surface of a brass column of standard size are removed by ultrasonic cleaning; the low-melting-point coating material is heated and melted in a quartz crucible, and a low-melting-point coating is formed on the surface within a specific length range of one end of the brass column of standard size by hot dipping; the thickness of the formed low-melting-point coating should be not less than 10 microns and not more than 50 microns, and the thickness of the low-melting-point coating should be uniform, the surface should be bright, and there should be no balling or weak wetting phenomenon;
[0065] Step 2: performing low-temperature aging treatment on the brass column with the low-melting-point coating formed on the surface, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the brass column / low-melting-point coating interface;
[0066] Step 3, printing an appropriate amount of solder paste on the array-arranged pads of the chip carrier substrate;
[0067] Similar to the traditional flip chip bumping process, a proper amount of solder paste is printed on the array pads of the chip carrier substrate using a template printing process, and the amount of solder paste printed on the array pads is required to be consistent;
[0068] Step 4, heating the solder paste to wet the array-arranged pads of the chip carrier substrate, and forming a spherical crown-shaped solder ball array with uniform shape and size on the array-arranged pads;
[0069] During the heating process, the flux in the solder paste is first activated and removes the oxide film on the surface of the pad through chemical reaction, and then the solder in the solder paste melts, wets the array-arranged pads, and forms a spherical crown-shaped solder ball array with a consistent height on the array-arranged pads of the chip carrier substrate under the action of surface tension;
[0070] Step 5: Welding of a brass column with a low melting point coating formed on a single surface:
[0071] Ultrasonic cleaning is used to remove impurities and oxides on the surface of a brass column with a low melting point coating formed on the surface; the brass column with a low melting point coating formed on the surface is clamped in a drill chuck of a micro-precision drilling machine, and the movement of a chip carrier substrate where a pad is located is controlled by a program so that the brass column with a low melting point coating formed on the surface is located above the pad and is aligned with the center of a solder ball on the pad; the brass column with a low melting point coating formed on the surface is driven by the drill chuck of the micro-precision drilling machine to rotate at a rotation speed of n1 and press downward, and wait until the low melting point coating is formed on the surface of the brass column. After the end of one end of the spot coating is in close contact with the top of the solder ball, the axial feeding of the brass column with a low-melting-point coating on the surface is stopped and its original rotation speed is maintained to preheat the contact surface between the two; after preheating for t1 time, the brass column with a low-melting-point coating on the surface is controlled to be axially pressed downward at a uniform feeding speed v1 and drill into the solder ball to a predetermined depth S; the axial feeding of the brass column with a low-melting-point coating on the surface is stopped and it is rotated at the original rotation speed for t2 time to perform heat preservation treatment on the solder point; then the brass column with a low-melting-point coating on the surface is made to rotate at the original rotation speed for t2 time to perform heat preservation treatment on the solder point; The coated brass column remains stationary to allow the solder joint to cool for t3 time; the drill chuck is opened and lifted, and the brass column with a low-melting-point coating on the surface remains in the spherical crown solder ball on the pad, completing the welding of a single brass column with a low-melting-point coating on the surface; during welding, the adhesion friction heat generation and interface temperature of the friction pair between the low-melting-point solder coating and the solder ball with similar performance are both high, and the low-melting-point coating at the interface of the friction pair is transformed into a thermoplastic state and then melted; the liquid low-melting-point coating solder flows, fills and wets the "barrel-shaped" friction pair interface of the solder ball under the action of axial, tangential and radial extrusion stresses during welding and forms a reliable friction brazing connection; the low-melting-point coating and the solder on both sides of the friction interface also undergo atomic mutual diffusion, adhesion and dynamic recrystallization during welding due to the heat-mechanical action they are subjected to, and there are plastic deformation connection mechanisms, diffusion connection mechanisms and recrystallization connection mechanisms between solid phase materials in the early stage of welding, and in the later stage of welding, it is transformed into a dissolution-diffusion connection mechanism of brazing between liquid and solid phases. Compared with the improved embedded friction welding method of copper pillars of CGA devices without mold-assisted positioning, no traces of the interface of the low-melting-point coating / brazine friction pair and no areas where substantial connection was not achieved were observed in the lower, middle and upper areas of the bottom and side surfaces of the brass pillars of the solder joints after welding.
[0072] Schematic diagram of the solder joint structure after friction brazing of a brass column with a low melting point coating on a single surface. Figure 2As shown, 11 is a chip carrier substrate; 12 is a solder pad on the chip carrier substrate; 13 is a solder resist film on the chip carrier substrate; 14 is a cylindrical brass column of standard size; 15 is a low-melting-point coating on the surface of the brass column; 16 is an intermetallic compound layer generated between the brass column and the low-melting-point coating; 17 is a spherical crown-shaped solder ball formed by the solder paste on the solder pad after reflow soldering; 18 is a crystallized area formed after the low-melting-point coating undergoes a melting and cooling solidification process during soldering.
[0073] Step 6: Connection of the brass column array with a low melting point coating formed on the surface:
[0074] Repeat the process of step 5 above with the same size parameters and process parameters, and weld the brass columns with a low-melting-point coating on the surface of each array-arranged pad on the chip carrier substrate one by one, and ensure that the exposed end height of the brass column array with a low-melting-point coating on the surface after welding is consistent.
[0075] The present invention can be used to achieve high-quality connection of surface array packaging devices with high frequency, high power and high reliability requirements in the fields of aerospace, communications, military industry, automotive electronics, etc. Specific implementation method three:
[0077] The copper pillar described in step 1 of this embodiment is any one of a pure copper pillar, a brass pillar, a tin bronze pillar, and a beryllium copper pillar of uniform specifications and sizes prepared according to standards; the aspect ratio of the copper pillar described in step 1 of this embodiment is in the range of 5 to 20, and the diameter d of the copper pillar is not less than 1 / 4 of the pad diameter D and not more than 2 / 5 of the pad diameter D; the low melting point coating described in step 1 of this embodiment is any one of BiInSn series, BiPbSn series, PbInSn series, SnBiInZn series, SnPbInBiSb series, SnIn series, and SnBi series soft solder coatings.
[0078] The other steps and parameters are the same as those in the first or second embodiment. Specific implementation method four:
[0080] The process for preparing the low-melting-point coating material described in step 1 of this embodiment is to first heat it to 40 to 60°C above the melting point of the metal with the highest melting point in the coating material components for melting, and then gradually reduce the heating temperature to 40 to 60°C above the eutectic point (or liquidus) of the coating material for melting, and the melting time is 10 to 40 minutes; the process temperature of the hot dipping described in step 1 of this embodiment is 35 to 60°C above the eutectic point (or liquidus) temperature of the coating material, and the hot dipping time is 30 to 120s; the hot dipping method described in step 1 of this embodiment is used to form a low-melting-point coating on the surface within a specific length range at one end of a copper column of standard size, the specific length range is 6d to 10d, d is the diameter of the copper column, and the thickness of the formed low-melting-point coating is 10 to 50 microns.
[0081] The other steps and parameters are the same as those in the first to third embodiments. Specific implementation method five:
[0083] The low-temperature aging temperature range of the copper pillar with a low-melting-point coating formed on the surface described in step 2 of this embodiment is 50°C to 100°C, and the low-temperature aging time is 0.5 to 6 hours; after low-temperature aging, the thickness of the intermetallic compound layer formed between the copper pillar / low-melting-point coating of the copper pillar with a low-melting-point coating formed on the surface described in step 2 of this embodiment is 1.0 to 2.5 microns.
[0084] The other steps and parameters are the same as those in Specific Embodiments 1 to 4. Specific implementation method six:
[0086] The type of the array-arranged pads described in step 3 of this embodiment is any one of a pure copper pad, a pure copper pad containing a Ni surface layer, and a pure copper pad containing an Au / Ni surface layer.
[0087] The other steps and parameters are the same as those in the first to fifth embodiments. Specific implementation method seven:
[0089] The type of solder in the solder paste described in step 4 of this embodiment is any one of SnCu, SnAg, SnAgCu, SnSb, SnBiAg, SnBiAgCu, and SnZnBi soft solders; the heating temperature of the solder paste described in step 4 of this embodiment is 30°C to 55°C above the eutectic point (or liquidus) temperature of the solder in the solder paste, and the height h of the formed array of spherical crown solder balls is greater than 7 / 10 of the pad diameter D.
[0090] The other steps and parameters are the same as those in the first to sixth embodiments. Specific implementation eight:
[0092] The exposed end length of the copper column with a low-melting-point coating on its surface, which is clamped in the drill chuck of a micro-precision drilling machine as described in step 5 of this embodiment, is 1.2 to 2.5 times the height h of the spherical crown solder ball; the rotation speed n1 of the copper column with a low-melting-point coating on its surface as described in step 5 of this embodiment ranges from 5000 rpm to 12000 rpm; the preheating time t1 of the copper column with a low-melting-point coating on its surface as described in step 5 of this embodiment to maintain the original rotation speed n1 is 5 seconds to 25 seconds.
[0093] The other steps and parameters are the same as those in the first to seventh embodiments. Specific implementation method nine:
[0095] The axial feed speed v1 of the copper column with a low-melting-point coating formed on the surface described in step 5 of this embodiment is in the range of 10 to 60 microns / second; the predetermined depth S described in step 5 of this embodiment is in the range of 0.6h to h-0.1mm, where h is the height of the array spherical crown solder balls.
[0096] The other steps and parameters are the same as those in any one of the specific implementation modes 1 to 8. Specific implementation method ten:
[0098] The range of the holding time t2 for stopping the axial feed of the copper column with a low-melting-point coating on the surface and rotating it at the original rotation speed described in step 5 of this embodiment is 5 to 30 seconds; the range of the cooling time t3 for keeping the copper column with a low-melting-point coating on the surface still described in step 5 of this embodiment is 15 to 60 seconds.
[0099] The other steps and parameters are the same as those in Specific Embodiments 1 to 9.
[0100] Example
[0101] Embodiment 1
[0102] Figure 3 The longitudinal section diagram of a single interconnected structure is shown in which one end of the pure copper column with a low melting point coating formed on the surface is connected by friction brazing, and then the other end of the pure copper column without coating is connected by low temperature reflow soldering. Wherein, A is a printed circuit board; B is a pad on the printed circuit board; C is a solder mask on the printed circuit board; D is a cylindrical pure copper column of standard size; E is a low melting point coating on the surface of the pure copper column; F is an intermetallic compound layer generated between the pure copper column and the low melting point coating; G is a spherical crown solder ball formed by the solder paste on the pad on the printed circuit board after reflow soldering; H is a crystallized area formed after the low melting point coating undergoes a melting and cooling solidification process during soldering; I is a chip carrier substrate; J is a pad on the chip carrier substrate; K is a solder mask on the chip carrier substrate; L is a solder fillet formed at the other end of the pure copper column without a low melting point coating formed on the surface after low temperature reflow soldering.
[0103] Taking the connection of pure copper columns in an array in a secondary package as an example, the welding process of a pure copper column array with a low-melting-point coating formed on the surface of a CGA device mainly includes: a first stage of welding one end of the array pure copper column surface with a low-melting-point coating formed on the surface of the array to the pads arranged in an array on a printed circuit board, and a second stage of low-temperature reflow soldering of the other end of the array pure copper column surface without a low-melting-point coating formed on the surface of the array to the pads arranged in an array on a chip carrier substrate and the solder paste thereon.
[0104] With respect to the welding process of forming a low melting point coating on the surface of the array pure copper column at one end in the first stage with the array-arranged pads of the printed circuit board, a friction brazing method for CGA device packaging according to the present invention comprises the following steps:
[0105] Step 1: Preparation of low melting point coating on the surface of pure copper column:
[0106] The pure metal raw materials of tin, bismuth and indium with a purity higher than 99.99% were weighed and mixed in a mass ratio of 32:49:19. -3 Pa vacuum high-frequency induction melting device to melt the alloy to form a low-melting-point 32Sn49Bi19In coating material with uniform composition and then cooled for standby use; preparing a cylindrical pure copper column of uniform specification size matching the diameter D of the printed circuit board pad, the diameter d of the pure copper column is D / 3, and the aspect ratio of the pure copper column is 11; ultrasonic cleaning is performed in an acetone solution for 5 minutes to remove impurities and oxide films on the surface of the pure copper column; hot dipping in a solution of the 32Sn49Bi19In coating material at a temperature of 150 to 170° C. for 60 seconds, forming a 32Sn49Bi19In coating with a thickness of 10 to 20 microns, a bright surface, no balling, and no weak wetting phenomenon on the surface of one end of a standard-sized pure copper column with a length range of 6d (d is the diameter of the pure copper column);
[0107] Step 2, performing a low-temperature aging treatment at 70° C. for 1.0 hour on the pure copper column with a low-melting-point 32Sn49Bi19In coating formed on the surface, so that a continuous scallop-shaped intermetallic compound layer with a thickness in the range of 1.0 to 2.5 μm is formed at the interface of the pure copper column / low-melting-point 32Sn49Bi19In coating;
[0108] Step 3: Print an appropriate amount of Sn1.0Cu solder paste on the pads arranged in an array on the printed circuit board using a template printing process, similar to the conventional BGA ball planting process. The amount of solder paste printed on the pad array should be kept consistent, and the height h of the Sn1.0Cu solder ball after reflow soldering should be approximately 1.0 times the pad diameter D.
[0109] Step 4, using a conventional reflow process curve with a peak temperature of 270° C. and a holding time of 60 seconds to heat the Sn1.0Cu solder paste on the array-arranged pure copper pads of the printed circuit board, so that the flux in the solder paste is first activated and the oxide film on the surface of the pure copper pads is removed by chemical reaction, and then the Sn1.0Cu solder in the solder paste is melted, wets the array-arranged pure copper pads, and forms a spherical crown solder ball array with a high degree of consistency on the array-arranged pure copper pads of the printed circuit board under the action of surface tension;
[0110] Step 5: Welding of a pure copper column with a low melting point 32Sn49Bi19In coating on a single surface:
[0111] Ultrasonic cleaning is used to remove impurities and oxides on the surface of a pure copper column with a low melting point 32Sn49Bi19In coating formed on the surface; the pure copper column with a low melting point coating formed on the surface is clamped in a drill chuck of a micro-precision drilling machine, the length of the exposed end of the pure copper column with a low melting point 32Sn49Bi19In coating formed on the surface is 1.3 times the height h of the solder ball, and the movement of a printed circuit board where a pad is located is controlled by a program so that the pure copper column with a low melting point 32Sn49Bi19In coating formed on the surface is located above the pad and aligned with the center of the solder ball on the pad; the pure copper column with a low melting point 32Sn49Bi19In coating formed on the surface is driven by the drill chuck of the micro-precision drilling machine to rotate and press down at a rotation speed of 8000 rpm, and after the end of one end of the pure copper column with a low melting point 32Sn49Bi19In coating formed on the surface is in close contact with the top of the solder ball, the axial rotation of the pure copper column with a low melting point 32Sn49Bi19In coating formed on the surface is stopped. Feed and maintain its original speed to preheat the contact surface between the two; after preheating for 10 seconds, control the pure copper column with a low melting point 32Sn49Bi19In coating on the surface to be uniformly pressed axially downward at a feed speed of 25 μm / s and drill into the interior of the Sn1.0Cu solder ball to a predetermined depth S=0.7h, where h is the height of the Sn1.0Cu solder ball; stop the axial feeding of the pure copper column with a low melting point 32Sn49Bi19In coating on the surface and make it rotate at 8000 The rotation speed of rpm is continued for 10 seconds to keep the solder joint warm; then the pure copper column with a low melting point 32Sn49Bi19In coating on the surface is kept still to allow the solder joint to cool for 30 seconds; the drill chuck is opened and lifted, and the pure copper column with a low melting point 32Sn49Bi19In coating on the surface is left in the spherical crown-shaped Sn1.0Cu solder ball on the pad, completing the welding of a single pure copper column with a low melting point 32Sn49Bi19In coating on the surface. During welding, the adhesion friction heat generation and interface temperature of the friction pair between the low-melting-point 32Sn49Bi19In coating and the Sn1.0Cu solder ball are both high. The low-melting-point 32Sn49Bi19In coating at the interface of the friction pair is transformed into a thermoplastic state and then melts. Under the action of axial, tangential and radial extrusion stresses during welding, the liquid low-melting-point 32Sn49Bi19In coating solder flows, fills and wets the "barrel-shaped" friction pair interface of the Sn1.0Cu solder ball, and forms a reliable friction brazing connection after cooling. Due to the thermal-mechanical action, the low-melting-point 32Sn49Bi19In coating and the Sn1.0Cu solder on both sides of the friction interface also undergo atomic mutual diffusion, adhesion and dynamic recrystallization during welding. In the early stage of welding, there are plastic deformation connection mechanisms, diffusion connection mechanisms and recrystallization connection mechanisms between solid phase materials, which are transformed into the dissolution-diffusion connection mechanism of brazing between liquid and solid phases in the later stage of welding.Compared with the improved embedded friction welding method of CGA device copper pillar without mold-assisted positioning, no traces of the interface of the low-melting-point coating / Sn1.0Cu solder friction pair and no areas where substantial connection was not achieved were observed on the bottom, middle and upper areas of the bottom and side surfaces of the pure copper pillar of the solder joint after welding.
[0112] Step 6: Connection of pure copper column array with low melting point 32Sn49Bi19In coating on the surface:
[0113] Repeat the process of step 5 above with the same size parameters and process parameters, and realize the welding of the pure copper columns with low melting point 32Sn49Bi19In coating formed on the surface of each array-arranged pure copper pad on the printed circuit board one by one, and ensure that the exposed end height of the pure copper column array with low melting point 32Sn49Bi19In coating formed on the surface after welding is consistent.
[0114] The above steps can realize the connection of one end of the pure copper column array with a low-melting-point 32Sn49Bi19In coating on the surface by the friction brazing method. The following steps are to realize the connection of the other end of the pure copper column array without a low-melting-point 32Sn49Bi19In coating on the surface by low-temperature reflow soldering: a proper amount of Sn2.0Ag0.5Cu7.5Bi solder paste is printed on the pure copper pads arranged in an array on the chip carrier substrate by a template printing method, and the Sn2.0Ag0.5Cu7.5Bi solder paste on the pure copper pads arranged in an array on the chip carrier substrate is heated by a traditional reflow soldering process curve with a peak temperature of 230°C and a holding time of 60 seconds. The flux in the solder paste is first activated and the oxide film on the surface of the pure copper pad is removed by chemical reaction. Then the melted Sn2.0Ag0.5Cu7.5Bi solder wets the pure copper pads arranged in an array and realizes the welding of the other end of the pure copper column array with a low-melting-point 32Sn49Bi19In coating on the surface.
[0115] During this period, the welding parts at both ends of the pure copper column array with a low-melting-point 32Sn49Bi19In coating formed on the surface are in the heating environment of reflow soldering, and the local area where the low-melting-point 32Sn49Bi19In coating of the aforementioned friction brazing joint is located will melt again on a larger scale. The secondary remelting of the friction interface can improve the insufficient filling or poor wetting of the "barrel-shaped" interface of the Sn1.0Cu solder ball by liquid 32Sn49Bi19In due to limited friction heat generation during friction brazing, thereby further improving the connection strength of the pure copper column friction brazing joint with a low-melting-point 32Sn49Bi19In coating formed on the surface.
[0116] Embodiment 2
[0117] Figure 4The longitudinal section of a single interconnected structure is a schematic diagram of a single interconnected structure after the end of the H96 brass column with a low melting point coating formed on the surface is connected by friction brazing, and then the other end of the H96 brass column without coating is connected by low temperature reflow soldering. Among them, AA is a chip carrier substrate; BB is a pad on the chip carrier substrate; CC is a solder mask on the chip carrier substrate; DD is a cylindrical H96 brass column of standard size; EE is a low melting point coating on the surface of the H96 brass column; FF is an intermetallic compound layer generated between the H96 brass column and the low melting point coating; GG is a spherical crown solder ball formed by the solder paste on the pad of the chip carrier substrate after reflow soldering; HH is a crystallized area formed after the low melting point coating undergoes a melting and cooling solidification process during soldering; II is a printed circuit board; JJ is a pad on the printed circuit board; KK is a solder mask on the printed circuit board; LL is a solder fillet formed at the other end of the H96 brass column without a low melting point coating formed on the surface after low temperature reflow soldering.
[0118] Taking the connection of the array H96 brass column in the secondary package as an example, the welding process of the H96 brass column array with a low-melting-point coating formed on the surface of the CGA device mainly includes: the first stage of the welding process of one end of the array H96 brass column surface with a low-melting-point coating formed on the chip carrier substrate and the array-arranged pads of the chip carrier substrate; and the second stage of the low-temperature reflow soldering process of the other end of the array H96 brass column surface without a low-melting-point coating formed on the printed circuit board and the solder paste thereon.
[0119] With respect to the welding process of forming a low melting point coating on the surface of the array H96 brass column at the first stage with the pads arranged in an array on the chip carrier substrate, a friction brazing method for CGA device packaging according to the present invention comprises the following steps:
[0120] Step 1: Preparation of low melting point coating on the surface of H96 brass column:
[0121] The pure metal raw materials of tin, bismuth and lead with a purity higher than 99.99% were weighed and mixed in a mass ratio of 25:46:29. -3The alloy is melted in a vacuum high-frequency induction melting device of Pa to form a low-melting-point 25Sn46Bi29Pb coating material with uniform composition and then cooled for standby use; a cylindrical H96 brass column of uniform specification size matching the diameter D of the chip carrier substrate pad is prepared, the diameter d of the H96 brass column is D / 4, and the aspect ratio of the pure copper column is 14; ultrasonic cleaning is performed in an acetone solution for 5 minutes to remove impurities and oxide films on the surface of the H96 brass column; hot-dip dipping is performed in a 25Sn46Bi29Pb coating material solution at a temperature of 160 to 190° C. for 80 seconds to form a 25Sn46Bi29Pb coating with a thickness of 12 to 25 microns, a bright surface, no balling, and no weak wetting phenomenon on the surface of one end of a standard-sized H96 brass column with a length range of 8d (d is the diameter of the H96 brass column);
[0122] Step 2, performing a low-temperature aging treatment at 80° C. for 1.5 hours on the H96 brass column with a low-melting-point 25Sn46Bi29Pb coating formed on the surface, so that a continuous scallop-shaped intermetallic compound layer with a thickness in the range of 0.8 to 2.0 μm is formed at the interface of the H96 brass column / low-melting-point 25Sn46Bi29Pb coating;
[0123] Step 3: Print an appropriate amount of Sn0.7Ag0.5Cu solder paste on the array pads of the chip carrier substrate using a template printing process, the same as the manufacturing process of the flip chip package bumps. It is required that the amount of solder paste printed on the pad array should be consistent, and the height h of the Sn0.7Ag0.5Cu solder ball after reflow soldering should be approximately 1.1 times the pad diameter D;
[0124] Step 4, using a conventional reflow process curve with a peak temperature of 260°C and a holding time of 55 seconds to heat the Sn0.7Ag0.5Cu solder paste on the array-arranged pure copper pads of the chip carrier substrate, so that the flux in the solder paste is first activated and the oxide film on the surface of the pure copper pads is removed by chemical reaction, and then the Sn0.7Ag0.5Cu solder in the solder paste is melted, wets the array-arranged pure copper pads, and forms a spherical crown solder ball array with a high degree of consistency on the array-arranged pure copper pads of the chip carrier substrate under the action of surface tension;
[0125] Step 5: Welding of H96 brass column with low melting point 25Sn46Bi29Pb coating on a single surface:
[0126] Ultrasonic cleaning is used to remove impurities and oxides on the surface of the H96 brass column with a low melting point 25Sn46Bi29Pb coating formed on the surface; the H96 brass column with a low melting point coating formed on the surface is clamped in the drill chuck of a micro precision drilling machine, the length of the exposed end of the H96 brass column with a low melting point 25Sn46Bi29Pb coating formed on the surface is 1.5 times the height h of the solder ball, and the chip carrier substrate where the solder pad is located is moved by program control, so that the H96 brass column with a low melting point 25Sn46Bi29Pb coating formed on the surface The column is located above the pad and aligned with the center of the solder ball on the pad; the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface is driven by the drill chuck of a micro precision drilling machine to rotate at a speed of 9000 rpm and press down, and after the end of one end of the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface is in close contact with the top of the Sn0.7Ag0.5Cu solder ball, the axis of the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface is stopped. The H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface is fed and maintained at its original speed to preheat the contact surface between the two; after preheating for 13 seconds, the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface is controlled to be uniformly pressed axially downward at a feeding speed of 30 μm / s and drilled into the interior of the Sn0.7Ag0.5Cu solder ball to a predetermined depth S=0.75h, where h is the height of the Sn0.7Ag0.5Cu solder ball; the axial feeding of the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface is stopped and made to rotate at 90 00 rpm and continue to rotate for 15 seconds to keep the solder joint warm; then keep the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface still to cool the solder joint for 40 seconds; open and lift the drill chuck and leave the H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface in the spherical crown Sn0.7Ag0.5Cu solder ball on the pad to complete the welding of a single H96 brass column with a low melting point 25Sn46Bi29Pb coating on the surface. During welding, the adhesive friction heat generation and interface temperature of the friction pair between the low-melting-point 25Sn46Bi29Pb coating and the Sn0.7Ag0.5Cu solder ball are both high. The low-melting-point 25Sn46Bi29Pb coating at the interface of the friction pair melts after transforming into a thermoplastic state. The liquid low-melting-point 25Sn46Bi29Pb coating solder flows, fills and wets the "barrel-shaped" friction pair interface of the Sn0.7Ag0.5Cu solder ball under the action of axial, tangential and radial extrusion stresses during welding, and forms a reliable friction brazing connection after cooling.The low melting point 25Sn46Bi29Pb coating and Sn0.7Ag0.5Cu solder on both sides of the friction interface also undergo atomic interdiffusion, adhesion, and dynamic recrystallization during welding due to the thermal-mechanical effects. In the early stage of welding, there are plastic deformation connection mechanisms, diffusion connection mechanisms, and recrystallization connection mechanisms between solid phase materials, which are transformed into dissolution-diffusion connection mechanisms of brazing between liquid and solid phases in the later stage of welding. Compared with the improved embedded friction welding method of CGA device copper pillars without mold-assisted positioning, no traces of the interface of the low melting point coating / solder friction pair and areas without substantial connection are observed in the bottom, middle, and upper areas of the bottom and side surfaces of the brass pillars of the solder joints after welding.
[0127] Step 6: Connection of H96 brass column array with low melting point 25Sn46Bi29Pb coating on the surface:
[0128] Repeat the process of step 5 above with the same size parameters and process parameters, and weld the H96 brass columns with a low melting point 25Sn46Bi29Pb coating on the surface of each array-arranged pure copper pad on the chip carrier substrate one by one, and ensure that the exposed end height of the H96 brass column array with a low melting point 25Sn46Bi29Pb coating on the surface after welding is consistent.
[0129] The above steps can realize the connection of one end of the H96 brass column array with a low-melting-point 25Sn46Bi29Pb coating on the surface by friction brazing method, and the following steps are to realize the connection of the other end of the array H96 brass column without a low-melting-point 25Sn46Bi29Pb coating on the surface by low-temperature reflow soldering: a proper amount of Sn7.5Zn3.0Bi solder paste is printed on the pure copper pads arranged in an array on the printed circuit board by a template printing method, and the Sn7.5Zn3.0Bi solder paste on the pure copper pads arranged in an array on the printed circuit board is heated by a traditional reflow soldering process curve with a peak temperature of 220°C and a holding time of 70 seconds. The flux in the solder paste is first activated and the oxide film on the surface of the pure copper pad is removed by chemical reaction, and then the melted Sn7.5Zn3.0Bi solder wets the pure copper pads arranged in an array and realizes the connection of the other end of the H96 brass column array with a low-melting-point 25Sn46Bi29Pb coating on the surface.
[0130] During this period, the connection parts at both ends of the H96 brass column array with a low-melting-point 25Sn46Bi29Pb coating formed on the surface are in the heating environment of reflow soldering, and the local area where the low-melting-point 25Sn46Bi29Pb coating of the aforementioned friction brazing joint is located will melt again on a larger scale. The secondary remelting of the friction interface can improve the insufficient filling or poor wetting of the "barrel-shaped" interface of the Sn0.7Ag0.5Cu solder ball by the liquid 25Sn46Bi29Pb coated solder due to limited friction heat generation during friction brazing, thereby further improving the connection strength of the friction brazing joint of the H96 brass column with a low-melting-point 25Sn46Bi29Pb coating formed on the surface.
Claims
1. A friction brazing method for CGA device packaging, characterized in that: The following steps are involved: Step 1: Preparation of low melting point coating on the surface of copper column: According to the designed ratio of various alloy elements, the low melting point coating material is prepared and the vacuum degree is 3×10 -3 The alloy is melted in a vacuum high-frequency induction melting device of Pa to form a low-melting-point coating material with uniform composition; the low-melting-point coating material is then heated and melted in a quartz crucible, and a low-melting-point coating is formed on the surface of a copper column of a standard size within a specific length range at one end thereof by a hot dip method; Step 2: performing low-temperature aging treatment on the copper pillar with the low-melting-point coating formed on the surface, so that a continuous intermetallic compound layer with suitable thickness and morphology is formed at the interface of the copper pillar / low-melting-point coating; Step 3: Print an appropriate amount of solder paste on the pads arranged in the array; Step 4, heating the solder paste to wet the array-arranged pads, and forming a spherical crown-shaped solder ball array with uniform shape and size on the array-arranged pads; Step 5: Welding of copper pillars with low melting point coating on a single surface: Ultrasonic cleaning is used to remove impurities and oxides on the surface of the copper column with a low melting point coating formed on the surface; the copper column with a low melting point coating formed on the surface is clamped in the drill chuck of a micro-precision drilling machine, and the movement of the substrate where the pad is located is controlled by a program so that the copper column with a low melting point coating formed on the surface is located above the pad and aligned with the center of the solder ball on the pad; the drill chuck of the micro-precision drilling machine is used to drive the copper column with a low melting point coating formed on the surface to rotate and press down at a rotation speed of n1, and after the end of one end of the copper column with a low melting point coating formed on the surface is in close contact with the top of the solder ball, the axial feeding of the copper column with a low melting point coating formed on the surface is stopped and its original rotation speed is maintained to preheat the contact surface between the two; after preheating for t1 time, the copper column with a low melting point coating formed on the surface is controlled to be axially pressed down at a uniform speed of v1 and drilled into a predetermined depth S inside the solder ball; the axial feeding of the copper column with a low melting point coating formed on the surface is stopped and it is rotated at the original rotation speed for t2 time to perform heat preservation treatment on the solder joint; Then, the copper pillar with the low melting point coating formed on the surface is kept still to allow the solder joint to cool for t3 time; The drill chuck is opened and lifted, and the copper column with a low-melting-point coating on the surface is left in the spherical crown-shaped solder ball on the pad, completing the welding of a single copper column with a low-melting-point coating on the surface; during welding, the adhesion friction heat generation and interface temperature of the friction pair between the low-melting-point solder coating and the solder ball with similar performance are both high, and the low-melting-point coating at the interface of the friction pair is transformed into a thermoplastic state and then melted; the liquid low-melting-point coating solder flows, fills and wets the "barrel-shaped" friction pair interface of the solder ball under the action of axial, tangential and radial extrusion stresses during welding. The friction pair interface is formed and a reliable friction brazing connection is formed; the low melting point coating and the brazing material on both sides of the friction interface also undergo atomic mutual diffusion, adhesion, and dynamic recrystallization during welding due to the thermal-mechanical action. In the early stage of welding, there are plastic deformation connection mechanisms, diffusion connection mechanisms, and recrystallization connection mechanisms between solid phase materials, which are transformed into dissolution-diffusion connection mechanisms of brazing between liquid and solid phases in the later stage of welding; after welding, no traces of the interface of the low melting point coating / brazing material friction pair and areas where no substantial connection is achieved are observed in the bottom, middle, and upper areas of the bottom and side surfaces of the copper column of the solder joint; Step 6: Welding of copper pillar array with low melting point coating on the surface: Repeat the process of step 5 above with the same size parameters and process parameters, and weld the copper pillars with low-melting-point coating on the surface of each array-arranged pad one by one, and ensure that the exposed end height of the copper pillar array with low-melting-point coating on the surface after welding is consistent.
2. A friction brazing method for CGA device packaging according to claim 1, characterized in that: The low melting point coating material described in step 1 is any one of BiInSn, BiPbSn, PbInSn, SnBiInZn, SnPbInBiSb, SnIn, and SnBi solders. The process for preparing the low melting point coating material described in step 1 is to first heat it to 40 to 60°C above the melting point (or liquidus) of the metal with the highest melting point in the coating material components for melting, and then gradually reduce the heating temperature to 40 to 60°C above the eutectic point (or liquidus) of the coating material for melting, and the melting time is 10 to 40 minutes.
3. A friction brazing method for CGA device packaging according to claim 2, characterized in that: The copper column described in step 1 is any one of a pure copper column, a brass column, a tin bronze column, and a beryllium copper column of uniform specifications and sizes prepared according to standards, the aspect ratio of the copper column ranges from 5 to 20, and the diameter d of the copper column is not less than 1 / 4 of the pad diameter D and not more than 2 / 5 of the pad diameter D.
4. A friction brazing method for CGA device packaging according to claim 3, characterized in that: The process temperature of the hot dipping described in step 1 is 35°C to 60°C above the eutectic point (or liquidus) temperature of the coating material, and the hot dipping time is 30 to 120s. The hot dipping method forms a low-melting-point coating on the surface within a specific length range at one end of a standard-sized copper column, the specific length range is 6d to 10d, d is the diameter of the copper column, and the thickness of the formed low-melting-point coating is 10 to 50 microns.
5. A friction brazing method for CGA device packaging according to claim 4, characterized in that: The low-temperature aging temperature range of the copper column with a low-melting-point coating formed on the surface in step 2 is 50°C to 100°C, the low-temperature aging time is 0.5 to 6 hours, and the thickness of the intermetallic compound layer formed between the copper column / low-melting-point coating after low-temperature aging is 1.0 to 2.5 microns.
6. A friction brazing method for CGA device packaging according to claim 5, characterized in that: The type of the array-arranged pads described in step 3 is any one of a pure copper pad, a pure copper pad containing a Ni surface layer, and a pure copper pad containing an Au / Ni surface layer.
7. A friction brazing method for CGA device packaging according to claim 6, characterized in that: The type of solder in the solder paste described in step 4 is any one of SnCu, SnAg, SnAgCu, SnSb, SnBiAg, SnBiAgCu, and SnZnBi soft solders. The heating temperature of the solder paste is 30°C to 55°C above the eutectic point (or liquidus) temperature of the solder in the solder paste. The height h of the spherical crown solder balls in the array formed is greater than 7 / 10 of the pad diameter D.
8. A friction brazing method for CGA device packaging according to claim 7, characterized in that: The exposed end length of the copper column with a low-melting-point coating on the surface of the copper column clamped in the drill chuck of the micro-precision drilling machine described in step 5 is 1.2 to 2.5 times the height h of the spherical crown solder ball, the rotation speed n1 of the copper column with a low-melting-point coating on the surface ranges from 5000 rpm to 12000 rpm, and the preheating time t1 of the copper column with a low-melting-point coating on the surface to maintain the original rotation speed n1 is 5 seconds to 25 seconds.
9. A friction brazing method for CGA device packaging according to claim 8, characterized in that: The axial feed speed v1 of the copper column with a low-melting-point coating on the surface described in step 5 ranges from 10 to 60 microns / second, and the predetermined depth S of the copper column with a low-melting-point coating on the surface drilling into the solder ball ranges from 0.6h to h-0.1mm, where h is the height of the array spherical crown solder balls.
10. A friction brazing method for CGA device packaging according to claim 9, characterized in that: The range of the holding time t2 for stopping the axial feeding of the copper column with a low-melting-point coating on the surface and rotating it at the original rotation speed described in step 5 is 5 to 30 seconds, and the range of the cooling time t3 for keeping the copper column with a low-melting-point coating on the surface still is 15 to 60 seconds.