Pseudo-boehmite / graphene powder, aluminum oxide / graphene coating, preparation method and application
Through the preparation of phthalinated alumina/graphene powder and plasma thermal spraying technology, the problems of poor dispersion of alumina/graphite composite coating and uneven phase distribution are solved, and high density and good friction performance are achieved. Alumina/graphene coating is suitable for friction reduction and wear resistance needs of large mechanical parts.
Patent Information
- Application Number
- CN202410996727.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
AI Technical Summary
The existing alumina/graphite composite coatings have poor dispersion and uneven phase distribution during powder preparation, resulting in insufficient friction reduction and wear resistance, and harsh operating conditions, affecting production efficiency and product quality.
The composite microspheres were prepared by using pseudothic aluminite/graphene powder, and the graphite was treated by prehydroxylation, dispersant was added and high-pressure homogeneous peeling was performed. Compound microspheres were prepared in combination with spray drying to form a uniformly distributed alumina/graphene coating. The plasma thermal spraying process is used to improve density and dispersion.
The alumina/graphene coating has achieved uniform phase distribution, strong bonding and good dispersion characteristics, improved friction performance and wear resistance, reduced friction coefficient, and simple process, environmental protection, low cost, suitable for Mass production.
Smart Images

Figure CN118894543A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and in particular to pseudo-boehmite / graphene powder, aluminum oxide / graphene coating, and preparation methods and applications thereof. Background Art
[0002] With the substantial increase in productivity, large-scale mechanical parts need to meet more demanding working environments, long life, and low energy consumption. The key to achieving the above problems lies in the formation of anti-friction and anti-wear coatings on the outer layer of the workpiece. Among them, alumina ceramic materials are widely used in coatings of large-scale mechanical parts due to their high hardness, good stability, and excellent wear resistance, oxidation resistance, and corrosion resistance. However, in actual working conditions, alumina is wear-resistant but not anti-friction, so it is necessary to add materials with lubricating properties to form anti-friction and anti-wear coatings. Among the many added phases, graphite materials have been widely studied due to their high toughness and lubricating properties. Alumina / graphite composites provide wear resistance while increasing friction reduction, so alumina / graphite composites are considered to be one of the most promising materials for promoting the rapid development of anti-friction and anti-wear coatings.
[0003] Iftikhar Ahmad et al. prepared an alumina / graphene composite material by combining chemical and physical methods. This method effectively improved the bonding between the two phases and improved the overall density of the coating. However, a large amount of surfactant needs to be added during the powder preparation process to improve the uneven dispersion of alumina / graphene, and the composite material is hot-pressed and filled with high temperature and high pressure as the driving force. This also leads to more stringent operating conditions and subsequent treatment problems for a large amount of dispersants. Therefore, the residual dispersant in the preparation method has an adverse effect on the friction and wear resistance of the coating and on the scale-up production.
[0004] Zhao et al. used nickel-coated graphite to add graphite to 3Al 2 O 3 -2SiO 2 The preparation of composite materials, this preparation method has relatively simple operating conditions and does not require the introduction of a large amount of dispersant. The results show that with the increase of the content of nickel-coated graphite, the porosity of the coating gradually decreases and the hardness decreases. When the content of nickel-coated graphite in the coating is 20%, the friction coefficient and wear rate of the coating reach the lowest. However, the introduction of graphite will inevitably lead to uneven phase distribution and easy high-temperature oxidation during the plasma spraying process, resulting in a poor deposition rate of the powder particles on the substrate surface, resulting in the failure of the coating under friction conditions due to the combined effects of plastic deformation, brittle fracture and flaking.
[0005] In summary, the friction reduction and wear resistance of the coating often depend on the structure, morphology, density and other related properties of the powder material. Therefore, the preparation of composite powder materials with good dispersibility and uniform phase distribution is the key to meeting the development trend of friction reduction and wear resistance coatings. However, the structural characteristics of the alumina particles themselves cannot be modified on the crystal surface using simple methods. This also leads to weak bonding between the two phases after adding graphite materials, uneven phase distribution, and low density of powder particles. Therefore, during the reaction process, the particle state and dispersibility of the aluminum source precursor itself have an important influence on the distribution of phases during the composite process and the density of the composite powder material during the granulation process, and the composite powder material has an important influence on the friction reduction, wear resistance and toughness of the later coating. Therefore, it is crucial to find a suitable treatment method to make the bonding between the two phases strong, the phase distribution uniform, and the dispersibility good, so as to improve the overall density and size uniformity of the particles during plasma spraying. Summary of the invention
[0006] In order to solve the technical problems in the prior art that the alumina / graphene coating has poor anti-friction performance, and the precursors used for coating spraying have uneven phase distribution, weak bonding, and poor dispersibility, the present invention proposes a pseudo-boehmite / graphene powder, an alumina / graphene coating, and a preparation method and application. The pseudo-boehmite / graphene powder prepared by the present invention has the characteristics of uniform phase distribution, strong bonding, and high dispersion; and the alumina / graphene coating prepared by plasma thermal spraying of the composite microspheres is denser, has uniform phase distribution, and has good friction performance. In addition, the preparation process of the present application does not require a large amount of chemical reagents, is green and environmentally friendly, and has a simple process.
[0007] To achieve the above object, the technical solution of the present invention is implemented as follows: A method for preparing pseudo-boehmite / graphene powder, comprising the following steps: (1) Pre-hydroxylation of graphite to obtain hydroxyl-rich graphite powder; (2) adding the hydroxyl-rich graphite powder obtained in step (1) into deionized water and a dispersant, and obtaining a hydroxyl-rich graphene slurry after high-pressure homogenization and exfoliation; (3) adding acid to the pseudo-boehmite aqueous solution to form a sol, thereby obtaining an aluminum sol; (4) The hydroxyl-rich graphene slurry prepared in step (2) is added to the aluminum sol in step (3), and pseudo-boehmite / graphene powder is prepared by spray drying.
[0008] The specific steps of the pre-hydroxylation treatment in the above step (1) are: subjecting graphite and an alkaline grinding aid to a pre-hydroxylation reaction under ball milling.
[0009] The alkaline grinding aids are NaOH, KOH and Ca(OH) 2 Any one or a mixture of several of the following; the mass ratio of graphite to alkaline grinding aid is (2-5):(1-3); the process conditions of ball milling are: bead to material ratio is (4-7):(1-3), the ball milling speed is 240-260rpm, and the time is 300-550min.
[0010] In the above step (2), the dispersant is any one of PVP, PVA and PEG or a mixture of several thereof; the mass ratio of the hydroxyl-rich graphite powder to deionized water is (1-6): (3-9), and the mass of the dispersant accounts for 2%-5% of the mass of the deionized water; the specific process of high-pressure homogenization stripping in the step (2) is: the number of homogenization cycles is 10-80 cycles, and the pressure parameter during homogenization is 300-1800 bar.
[0011] In the above step (3), the concentration of the pseudo-boehmite aqueous solution is 200-900 g / L; the pH value of the sol is 1-6.
[0012] The mass ratio of the hydroxyl-rich graphene slurry to the aluminum sol in the above step (4) is (1-4): (2-9); the process conditions of the spray drying method are: inlet temperature 80-300°C, outlet temperature 50-150°C, feed speed 10-200 rpm, and atomizer speed 10000-30000 r / min.
[0013] Pseudo-boehmite / graphene powder prepared by the above preparation method.
[0014] Furthermore, the pseudo-boehmite / graphene powder presents a microsphere structure, in which the pseudo-boehmite grains form a protective layer on the outer layer, and the graphene wraps / rolls around the pseudo-boehmite grains to form an inner layer.
[0015] A method for preparing an aluminum oxide / graphene coating comprises the following steps: performing plasma thermal spraying on a substrate with the pseudo-boehmite / graphene powder to obtain the aluminum oxide / graphene coating.
[0016] The aluminum oxide / graphene coating is prepared by the above-mentioned preparation method.
[0017] The above-mentioned application of alumina / graphene coating in large mechanical parts.
[0018] The beneficial effects produced by the present invention are: (1) The present invention uses the pseudo-boehmite sol obtained after acid treatment as the aluminum source, which has higher reactivity, better dispersibility and smaller particle size than pure alumina as the aluminum source. By combining with hydroxylated graphene, it can avoid uneven phase distribution, poor microstructure and poor dispersibility. The hydrogen bonds and strong viscosity in the pseudo-boehmite sol make the graphene firmly wrapped / rolled around the AlO (OH) grains, and firmly fix several grains together in the form of hydrogen bonds, so that the prepared composite microspheres have a higher density. The porosity of the coating prepared by plasma thermal spraying process using pseudo-boehmite / graphene powder as raw material is 2.6%, which is much lower than 5.3% of the pure alumina coating, and at the same time gives the coating excellent density. In addition, the graphene material is evenly dispersed in the final overall coating to prevent the graphene flakes from peeling off, thereby making the coating have good anti-friction and anti-wear properties.
[0019] (2) The pseudo-boehmite / graphene powder prepared by the present invention presents a microsphere structure, in which the pseudo-boehmite grains form a protective layer on the outer layer, and the graphene wraps / rolls around the pseudo-boehmite grains to form an inner layer. There is almost no carbon element on the surface of the microsphere, and the pseudo-boehmite sol particles form a protective layer on the outer layer, which effectively protects the graphene from being oxidized by high temperature during the plasma spraying process, thereby improving the overall anti-friction performance of the coating, and its friction coefficient can be reduced to 0.32.
[0020] (3) The preparation method of pseudo-boehmite / graphene powder and alumina / graphene coating proposed in the present invention is green and environmentally friendly, has a simple process, low preparation cost, and is easy to mass produce, thereby avoiding the use of a large amount of organic solvents in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a SEM image of the exfoliated graphene material prepared in the present invention.
[0023] Figure 2 The stability analysis diagram of graphene slurries with different hydroxyl contents prepared in the present invention in water, wherein (a) is the hydroxylated graphite prepared in Example 1, (b) is the hydroxylated graphite prepared in Example 2, (c) is the unhydroxylated graphite of Comparative Example 2, (d) is the clarification index change curve, and (e) is the average value of the clarification index.
[0024] Figure 3 The Tyndall effect (a) and TEM morphology (b) of the aluminum sol prepared in the present invention.
[0025] Figure 4 This is a SEM image of the pseudo-boehmite / graphene powder prepared in the present invention.
[0026] Figure 5 The ultraviolet spectrum (a) of graphene prepared in Example 1, Example 2 and Comparative Example 2 of the present invention and the infrared spectrum (b) of pseudo-boehmite / graphene powder.
[0027] Figure 6 SEM images of the surface (a) and interior (b) of the pseudo-boehmite / graphene powder prepared in the present invention and their corresponding mapping images.
[0028] Figure 7 X-ray diffraction patterns of the composite materials prepared in Examples 1-4 of the present invention, wherein (a) is pseudo-boehmite / graphene powder, and (b) is an alumina / graphene coating after plasma thermal spraying.
[0029] Figure 8 The friction coefficient and wear rate of the aluminum oxide / graphene coatings of Examples 1-4 of the present invention and the aluminum oxide coating prepared in Comparative Example 1 under the conditions of 1N and 20HZ.
[0030] Fig. 9 These are the test curves of friction coefficient (a) and wear rate (b) of the aluminum oxide / graphene coating prepared in Example 2 and the pure aluminum oxide coating prepared in Comparative Example 1 under different loads.
[0031] Fig.10 (a) is a SEM image of the aluminum oxide / graphene coating prepared in Example 2 of the present invention, and (b) is a SEM image of the pure aluminum oxide coating of Comparative Example 1.
[0032] Fig.11 This is a mapping diagram of the aluminum oxide / graphene coating prepared in the present invention. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Mix 200g of graphite (5 microns) and 200g of alkaline grinding aid (Ca(OH) 2 ) is placed in a planetary ball mill, the bead-to-material ratio is controlled to be 4:1, the speed of the planetary ball mill is 240 rpm, and the ball milling time is 300 min to pre-hydroxylate it; the pre-hydroxylated graphite is dissolved in deionized water, and the hydrochloric acid solution is slowly added to the graphite solution, and the excess calcium hydroxide is washed clean and filtered.
[0035] (2) Dissolve 200 g of the washed hydroxylated graphite in 1500 g of deionized water and 30 g of PVP dispersant, and perform high-pressure homogenization and stripping under the conditions of 20 peeling cycles, 1000 bar of pressure, and 8 mL / s of flow rate to obtain a hydroxyl-rich graphene slurry.
[0036] (3) adding hydrochloric acid to the pseudo-boehmite aqueous solution (concentration of 357.14 g / L) until the pH value is 3.78, and performing sol formation to obtain aluminum sol; (4) 1700 g of the hydroxyl-rich graphene slurry obtained in step (2) was added to 5700 g of the aluminum sol obtained in step (3), and the pseudo-boehmite / graphene powder was obtained by spray drying under the conditions of an inlet air temperature of 150°C, an outlet air temperature of 87°C, a feed rate of 40 rpm, and an atomizer speed of 12600 r / min, and was recorded as Al-C-1.
[0037] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0038] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. Among them, the plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating (aluminum oxide / graphene coating) is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0039] Example 2 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Mix 200g of graphite (5 microns) and 100g of alkaline grinding aid (Ca(OH) 2 ) is placed in a planetary ball mill, the bead-to-material ratio is controlled to be 4:1, the speed of the planetary ball mill is 240 rpm, and the ball milling time is 300 min to pre-hydroxylate it; the pre-hydroxylated graphite is dissolved in deionized water, and the hydrochloric acid solution is slowly added to the graphite solution, and the excess calcium hydroxide is washed clean and filtered.
[0040] (2) Dissolve 200 g of the washed hydroxylated graphite in 1500 g of deionized water and 30 g of PVA dispersant, and perform high-pressure homogenization and stripping under the conditions of 20 peeling cycles, 1000 bar of pressure, and 8 mL / s of flow rate to obtain a hydroxyl-rich graphene slurry.
[0041] (3) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 357.14 g / L) until the pH value is 4.12, and performing sol formation to obtain aluminum sol; (4) 1700 g of the hydroxyl-rich graphene slurry prepared in step (2) was added to 5700 g of the aluminum sol prepared in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 150°C, an outlet air temperature of 87°C, a feed rate of 40 rpm, and an atomizer speed of 12600 r / min, denoted as Al-C-2.
[0042] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0043] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0044] Example 3 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Mix 200g of graphite (45 microns) and 100g of alkaline grinding aid (Ca(OH) 2 ) is placed in a planetary ball mill, the bead-to-material ratio is controlled to be 4:1, the speed of the planetary ball mill is 240 rpm, and the ball milling time is 300 min to pre-hydroxylate it; the pre-hydroxylated graphite is dissolved in deionized water, and the hydrochloric acid solution is slowly added to the graphite solution, and the excess calcium hydroxide is washed clean and filtered.
[0045] (2) Dissolve 200 g of the washed hydroxylated graphite in 1500 g of deionized water and 30 g of PVA dispersant, perform high pressure homogenization and stripping under the conditions of 20 peeling cycles, 1000 bar pressure, and 8 mL / s flow rate, to obtain a hydroxyl-rich graphene slurry.
[0046] (3) adding dilute sulfuric acid to the pseudo-boehmite aqueous solution (concentration of 357.14 g / L) to a pH value of 3.98, and performing sol formation to obtain aluminum sol; (4) 1700 g of the hydroxyl-rich graphene slurry obtained in step (2) was added to 5700 g of the aluminum sol obtained in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 150°C, an outlet air temperature of 87°C, a feed speed of 40 rpm, and an atomizer speed of 12600 r / min, denoted as Al-C-3.
[0047] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0048] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0049] Example 4 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Mix 200g of graphite (45 microns) and 200g of alkaline grinding aid (Ca(OH) 2 ) is placed in a planetary ball mill, the bead-to-material ratio is controlled to be 4:1, the speed of the planetary ball mill is 240rpm, and the ball milling time is 300min to pre-hydroxylate it; the pre-hydroxylated graphite is dissolved in deionized water, and the hydrochloric acid solution is slowly added to the graphite solution, and the excess calcium hydroxide is washed clean and filtered.
[0050] (2) Dissolve 200 g of the washed hydroxylated graphite in 1500 g of deionized water and 30 g of PVA dispersant, perform high pressure homogenization and stripping under the conditions of 20 peeling cycles, 1000 bar pressure, and 8 mL / s flow rate, to obtain a hydroxyl-rich graphene slurry.
[0051] (3) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 357.14 g / L) to a pH value of 3.96, and performing sol formation to obtain an aluminum sol; (4) 1700 g of the hydroxyl-rich graphene slurry prepared in step (2) was added to 5700 g of the aluminum sol prepared in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 150°C, an outlet air temperature of 87°C, a feed speed of 40 rpm, and an atomizer speed of 12600 r / min, which was recorded as Al-C-4.
[0052] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0053] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0054] Example 5 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Place 200 g of graphite (5 μm) and 120 g of alkaline grinding aid (NaOH) in a planetary ball mill, control the bead-to-material ratio to 4:3, the speed of the planetary ball mill to 260 rpm, and the ball milling time to 550 min to pre-hydroxylate the graphite; dissolve the pre-hydroxylated graphite in deionized water, slowly add hydrochloric acid solution to the graphite solution, wash out the excess sodium hydroxide, and filter.
[0055] (2) Dissolve 150 g of the washed hydroxylated graphite in 450 g of deionized water and 22.5 g of PVP dispersant, and homogenize under high pressure with 80 peeling cycles, 1800 bar of pressure, and 8 mL / s of flow rate to obtain a hydroxyl-rich graphene slurry.
[0056] (3) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 900 g / L) to a pH value of 6, and performing sol formation to obtain an aluminum sol; (4) 500 g of the hydroxyl-rich graphene slurry prepared in step (2) was added to 1000 g of the aluminum sol prepared in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 300°C, an outlet air temperature of 150°C, a feed rate of 200 rpm, and an atomizer speed of 30,000 r / min, denoted as Al-C.
[0057] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0058] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0059] Example 6 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Place 200 g of graphite (5 μm) and 40 g of alkaline grinding aid (NaOH) in a planetary ball mill, control the bead-to-material ratio to 7:1, the speed of the planetary ball mill to 250 rpm, and the ball milling time to 400 min to pre-hydroxylate the graphite; dissolve the pre-hydroxylated graphite in deionized water, slowly add hydrochloric acid solution to the graphite solution, wash away excess calcium hydroxide, and filter.
[0060] (2) Dissolve 200 g of the washed hydroxylated graphite in 1800 g of deionized water and 45 g of PVA dispersant, and perform high-pressure homogenization and stripping under the conditions of 10 peeling cycles, 300 bar pressure, and 8 mL / s flow rate to obtain a hydroxyl-rich graphene slurry.
[0061] (3) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 200 g / L) until the pH value is 1.12, and performing sol formation to obtain aluminum sol; (4) 1700 g of the hydroxyl-rich graphene slurry prepared in step (2) was added to 850 g of the aluminum sol prepared in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 80°C, an outlet air temperature of 50°C, a feed rate of 10 rpm, and an atomizer speed of 10,000 r / min, denoted as Al-C.
[0062] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0063] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0064] Example 7 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Place 200 g of graphite (5 μm) and 300 g of alkaline grinding aid (NaOH) in a planetary ball mill, control the bead-to-material ratio to 7:3, the speed of the planetary ball mill to 240 rpm, and the ball milling time to 300 min to pre-hydroxylate the graphite; dissolve the pre-hydroxylated graphite in deionized water, slowly add hydrochloric acid solution to the graphite solution, wash away excess calcium hydroxide, and filter.
[0065] (2) Dissolve 200 g of the washed hydroxylated graphite in 100 g of deionized water and 5 g of PVA dispersant, and perform high-pressure homogenization and stripping under the conditions of 50 peeling cycles, 1000 bar of pressure, and 8 mL / s of flow rate to obtain a hydroxyl-rich graphene slurry.
[0066] (3) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 357.14 g / L) until the pH value is 4.12, and performing sol formation to obtain aluminum sol; (4) 200 g of the hydroxyl-rich graphene slurry prepared in step (2) was added to 1800 g of the aluminum sol prepared in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 200°C, an outlet air temperature of 100°C, a feed rate of 160 rpm, and an atomizer speed of 20,000 r / min, denoted as Al-C.
[0067] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0068] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0069] Example 8 The preparation method of pseudo-boehmite / graphene powder in this embodiment comprises the following steps: (1) Place 200 g of graphite (5 μm) and 300 g of alkaline grinding aid (NaOH) in a planetary ball mill, control the bead-to-material ratio to 7:3, the speed of the planetary ball mill to 240 rpm, and the ball milling time to 300 min to pre-hydroxylate the graphite; dissolve the pre-hydroxylated graphite in deionized water, slowly add hydrochloric acid solution to the graphite solution, wash away excess calcium hydroxide, and filter.
[0070] (2) Dissolve 200 g of the washed hydroxylated graphite in 300 g of deionized water and 15 g of PVA dispersant, and homogenize under high pressure with a peeling cycle of 50, a pressure of 1000 bar, and a flow rate of 8 mL / s to obtain a hydroxyl-rich graphene slurry.
[0071] (3) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 500 g / L) to a pH value of 4.12, and performing sol formation to obtain an aluminum sol; (4) 200 g of the hydroxyl-rich graphene slurry prepared in step (2) was added to 450 g of the aluminum sol prepared in step (3), and the pseudo-boehmite / graphene powder was prepared by spray drying under the conditions of an inlet air temperature of 150°C, an outlet air temperature of 87°C, a feed rate of 40 rpm, and an atomizer speed of 12600 r / min, denoted as Al-C.
[0072] The preparation method of the aluminum oxide / graphene coating of this embodiment comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0073] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0074] Comparative Example 1 The preparation method of the aluminum oxide coating of this comparative example comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0075] (b) Alumina powder (particle size 50 microns) was sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by plasma thermal spraying process to obtain an alumina coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating were: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating was: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0076] Comparative Example 2 The preparation method of pseudo-boehmite / graphene powder in this comparative example is different from that in Example 1 in that the graphite is not modified by hydroxylation, and the specific steps are as follows: (1) 200 g of graphite (5 μm) was dissolved in 1500 g of deionized water and 30 g of PVA dispersant. The number of peeling circles during homogenization was 20, the pressure parameter during homogenization was 1000 bar, and the flow rate parameter was 8 mL / s. High-pressure homogenization and peeling were performed for later use to obtain graphene slurry.
[0077] (2) adding dilute sulfuric acid to a pseudo-boehmite aqueous solution (concentration of 357.14 g / L) until the pH value is 4.12, and performing sol formation to obtain aluminum sol; (3) 1700 g of the graphene slurry prepared in step (2) was added to 5700 g of the aluminum sol prepared in step (3), and pseudo-boehmite / graphene powder was prepared by spray drying, i.e., under the conditions of an inlet air temperature of 150°C, an outlet air temperature of 87°C, a feed speed of 40 rpm, and an atomizer speed of 12600 r / min.
[0078] The preparation method of the aluminum oxide / graphene coating of this comparative example comprises the following steps: (a) Using 20 mm × 12 mm × 12 mm 316L stainless steel as the substrate, the substrate was first sandblasted using a GS-943 sandblasting machine (Beijing Changkong Sandblasting Equipment Co., Ltd.) to ensure better bonding between the coating and the substrate. The sandblasted substrate was then ultrasonically cleaned in acetone to remove impurities on the substrate surface. Before preparing the coating, a Ni-24.5Cr-6Al-0.4Y metal bonding layer with a thickness of about 100 µm was deposited on the sandblasted 316L metal substrate.
[0079] (b) The pseudo-boehmite / graphene powder prepared in this embodiment is sprayed onto the substrate containing the Ni-24.5Cr-6Al-0.4Y metal bonding layer prepared in step (a) by a plasma thermal spraying process to obtain an aluminum oxide / graphene coating with a thickness of 300 µm. The plasma thermal spraying process parameters for the bonding coating are: voltage 72V, current 600A, argon flow rate 57L / h, hydrogen flow rate 8L / h, delivery energy 42.5kW, spraying angle 90°, and the top coating is: voltage 70V, current 600A, argon flow rate 50L / h, hydrogen flow rate 9L / h, delivery energy 42.5kW, spraying angle 90°.
[0080] Test Case The hydroxylated graphite, aluminum sol, pseudo-boehmite / graphene powder and aluminum oxide / graphene coating prepared in the present invention were tested and analyzed, and the results are as follows.
[0081] Figure 1This is a SEM image of the exfoliated graphene material prepared in the present invention. It can be seen from the image that the hydroxylated graphite is exfoliated and homogenized to obtain graphene sheets with relatively uniform layers and good dispersion.
[0082] The stability of graphene slurries with different hydroxyl contents in water was tested. The specific test process is as follows: the graphene slurries in Example 1, Example 2 and Comparative Example 2 were selected, 20 μL of the three graphene slurries were taken respectively, and 70 mL of deionized water was taken for dilution treatment respectively to obtain three diluted graphene solvents, which were placed in a stability analyzer (LUMlumisizer651, LUM Instrument Company, Germany) for testing. Test conditions: the sample test tube was selected as LUM 10 mm, PA, Rect. Synthetic Cell (110-135xx), the contour line was 300, the time was an interval of 5S, the speed was 500 speed, the light factor was 1.00, and the temperature was 25.0°C. Figure 2 The stability analysis diagram of graphite with different hydroxyl contents in solution of the present invention, wherein (a) is the hydroxylated graphite prepared in Example 1, (b) is the hydroxylated graphite prepared in Example 2, (c) is the non-hydroxylated graphite prepared in Comparative Example 2, (d) is the clarification index change curve, and (e) is the average value of the clarification index. It can be seen from the figure that when the mass ratio of graphite to grinding aid is 2:1 (Example 2), the prepared hydroxylated graphite has higher stable dispersibility in solution. The reason is that when the content of the grinding aid is relatively high (Example 1), it will protect the graphite during the ball milling process, reduce the efficiency of pre-hydroxylization, and lead to reduced stable dispersibility in the solvent.
[0083] Figure 3 The Tyndall effect (a) and TEM morphology (b) of the aluminum sol prepared in the present invention. As can be seen from the figure, in the process of aluminum source sol, a large number of nano-scale microsphere sol particles with uniform size are observed to be formed by TEM (the area in the red line in Figure b), and at the same time, due to the uniform dispersion of the sol particles, an obvious Tyndall effect phenomenon (a) is produced.
[0084] Figure 4 This is a SEM image of the pseudo-boehmite / graphene powder prepared in the present invention. It can be seen from the image that the pseudo-boehmite / graphene powder presents a larger microsphere particle size, and the composite microsphere is relatively dense, the microsphere particle size is 25-70μm, the particles are uniform and have high particle fluidity.
[0085] Figure 5 The UV spectra (a) of graphene prepared in Example 1, Example 2 and Comparative Example 2 of the present invention and the infrared spectra (b) of pseudo-boehmite / graphene powder. Figure 5As can be seen in (a), a significant shift in the characteristic peak representing graphite is observed around 260nm, indicating that the modified graphene surface contains hydroxyl functional groups. Figure 5 (b) The composite microspheres prepared in Example 2 show that the -1 A decrease in the stretching vibration frequency of OH (red shift phenomenon) was observed near 1070 cm -1 A decrease in the stretching vibration frequency representing the out-of-plane bending of CH was observed nearby, indicating that the aluminum sol is linked to the hydroxyl-rich graphene through hydrogen bonds.
[0086] Figure 6 The SEM images of the surface (a) and interior (b) of the pseudo-boehmite / graphene powder prepared by the present invention and their corresponding mapping images. From the SEM mapping image (a), it can be seen that there is almost no C element on the surface of the composite microsphere, and the aluminum sol particles form a protective layer on the outer layer, which effectively protects the graphene from high-temperature oxidation during the plasma spraying process. The composite microsphere is cut and observed. The internal SEM mapping image (b) shows that the C element and the Al element are evenly distributed. The graphene sheet and the Al element are marked in the figure. Figure 5 (b) The combination confirms that graphene is firmly wrapped / rolled around the AlO(OH) crystals and linked by hydrogen bonds. Pseudoboehmite forms positively charged sol particles (AlO + ), the sol particles are repelled by the same charges, resulting in uniform dispersion. The surface of the modified graphene slurry is rich in hydroxyl functional groups, which makes the pseudo-boehmite sol particles smaller in size after the two substances are fully and evenly mixed. The modified single graphene layer is used as a carrier to connect and wrap around it by hydrogen bonding and viscosity. During the spray drying process, many micro-nano layer structures are compounded to obtain a microsphere structure. Therefore, the pseudo-boehmite grains in the microsphere structure form a protective layer on the outer layer, and the graphene wraps / rolls around the pseudo-boehmite grains to form an inner layer.
[0087] Figure 7 The X-ray diffraction diagram of the composite material prepared in Examples 1-4 of the present invention, wherein (a) is pseudo-boehmite / graphene powder, and (b) is the alumina / graphene coating after plasma thermal spraying. It can be seen from the figure that the composite material of aluminum sol and graphene prepared in the present invention undergoes a phase transformation after spraying to generate γ-Al 2 O 3 ,α-Al 2 O 3 and solid lubricating coatings of graphene.
[0088] The specific detection method of the friction coefficient is as follows: The coatings prepared in Examples 1-4 and the aluminum oxide coating prepared in Comparative Example 1 were subjected to dry friction tests in a reciprocating friction mode on a UMT-3MT friction tester. The specific friction conditions were: room temperature, relative humidity of 20±5%, vibration frequency of 20 Hz, amplitude of 2.5 mm, load of 1 N, friction time of 35 min, total sliding distance of 420 m, and the friction coefficient was measured.
[0089] The specific detection method of wear rate is as follows: A stainless steel ball with a diameter of 6 mm was selected and tested under the same conditions as the friction test. The wear volume was detected using a Micro-XAM-3D non-contact surface profiler (ADE Corporation, Massachusetts, USA). The coating wear rate (W, mm3·N-1m-1) was calculated using the formula W=V / PL, where V is the wear volume of the coating in mm 3 , P is the applied load in N, L is the total sliding distance in m. The wear scar diameter of the 316L stainless steel ball was measured with an Olympus microscope with an accuracy of 0.01 mm. The wear volume (Vb) of the dual ball was calculated by the formula Vb= πρ4 / 4r, where ρ is the radius of the wear scar in mm, and r is the radius of the ball in mm. Finally, the wear rate (Wb) of the dual ball was obtained according to the formula Wb=Vb / PL.
[0090] Figure 8 The friction performance diagram of the aluminum oxide / graphene coating prepared in Examples 1-4 of the present invention and the aluminum oxide coating prepared in Comparative Example 1 under the conditions of 1N and 20HZ can be seen from the test of the friction coefficient and wear rate in the figure that the composite microsphere coating has a higher wear resistance than the pure Al 2 O 3 When the sacrificial part of the coating is worn, the friction coefficient of Example 2 is 0.32, which is 1.5 times lower than the friction coefficient of Comparative Example 1 of 0.81. Under the same other conditions, the wear rate of Example 2 is 6.49×10 -5 mm 3 ·(N·m) -1 , through Figure 2 Combined with the verification, it can be inferred that under the conditions of Example 2, the dispersion performance of graphene is the best and the microspheres composited with aluminum sol have the best effect.
[0091] The aluminum oxide / graphene coating prepared in Example 2 and the pure aluminum oxide coating prepared in Comparative Example 1 were subjected to friction and wear tests under different loads. The results are as follows: Fig. 9It can be seen that the friction coefficient of the coating in Example 2 decreases from the initial 0.32 to 0.27 when the load increases. As the load continues to increase, the graphene forms a dense carbon transfer film, which makes the Al pulled out of the coating during the friction process 2 O 3 There are fewer hard particles, and the wear rate is reduced from the initial 6.49×10 -5 mm 3 ·(N·m) -1 Reduced to 2.62×10 -5 mm 3 ·(N·m) -1 .
[0092] Fig.10 (a) is the SEM image of the alumina / graphene coating of Example 2 of the present invention, and (b) is the SEM image of the pure alumina coating of Comparative Example 1. It can be seen from the figure that the surface of the coatings is in a partially molten state and has a thin pancake shape. Both coatings are composed of completely molten areas and partially molten particles and have pores (marked in red). The microscope image analysis method is used to take images of the two coatings, and then the software analysis is used to select the pore area of x mm 2 , total coating area 100 mm 2 Substituting into the formula, the porosity is calculated as x / 100×100%. The porosity of the coating of Example 2 is 2.6%, while the porosity of the pure alumina coating of Comparative Example 1 is 5.3%. Therefore, the coating of Example 2 has higher density.
[0093] Fig.11 This is a mapping diagram of the aluminum oxide / graphene coating prepared by the present invention, which is Figure 6 The combination shows that due to the uniform distribution and high density of C and Al elements inside the microspheres, effective deposition during the thermal spraying process leads to uniform element distribution of the entire coating.
[0094] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing pseudo-boehmite / graphene powder, characterized in that: Here are the steps: (1) Pre-hydroxylating graphite to obtain hydroxyl-rich graphite powder; (2) adding the hydroxyl-rich graphite powder obtained in step (1) into deionized water and a dispersant, and obtaining a hydroxyl-rich graphene slurry after high-pressure homogenization and exfoliation; (3) adding acid to the pseudo-boehmite aqueous solution to form a sol to obtain an aluminum sol; (4) The hydroxyl-rich graphene slurry prepared in step (2) is added to the aluminum sol in step (3), and pseudo-boehmite / graphene powder is prepared by spray drying.
2. The method for preparing pseudo-boehmite / graphene powder according to claim 1, characterized in that: The specific steps of the pre-hydroxylation treatment in step (1) are: subjecting graphite and an alkaline grinding aid to a pre-hydroxylation reaction under ball milling.
3. The method for preparing pseudo-boehmite / graphene powder according to claim 2, characterized in that: The alkaline grinding aid is any one of NaOH, KOH and Ca(OH)2 or a mixture of several thereof; the mass ratio of graphite to alkaline grinding aid is (2-5):(1-3); the process conditions of ball milling are: the bead to material ratio is (4-7):(1-3), the ball milling speed is 240-260rpm, and the time is 300-550min.
4. The method for preparing pseudo-boehmite / graphene powder according to claim 2, characterized in that: In the step (2), the dispersant is any one of PVP, PVA and PEG or a mixture of several thereof; the mass ratio of the hydroxyl-rich graphite powder to deionized water is (1-6): (3-9), and the mass of the dispersant accounts for 2%-5% of the mass of the deionized water; the specific process of high-pressure homogenization stripping is: the number of homogenization circles is 10-80 circles, and the pressure parameter during homogenization is 300-1800 bar.
5. The method for preparing pseudo-boehmite / graphene powder according to claim 4, characterized in that: The concentration of the pseudo-boehmite aqueous solution in step (3) is 200-900 g / L; the pH value of the sol is 1-6.
6. The method for preparing pseudo-boehmite / graphene powder according to claim 5, characterized in that: The mass ratio of the hydroxyl-rich graphene slurry to the aluminum sol in the step (4) is (1-4): (2-9); the process conditions of the spray drying method are: inlet temperature 80-300°C, outlet temperature 50-150°C, feed speed 10-200 rpm, and atomizer speed 10000-30000 r / min.
7. Pseudo-boehmite / graphene powder prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The pseudo-boehmite / graphene powder presents a microsphere structure, in which the pseudo-boehmite grains form a protective layer on the outer layer, and the graphene wraps / rolls around the pseudo-boehmite grains to form an inner layer.
8. A method for preparing an aluminum oxide / graphene coating, characterized in that: The steps are: plasma thermal spraying the pseudo-boehmite / graphene powder described in claim 7 on a substrate to obtain an aluminum oxide / graphene coating.
9. Aluminum oxide / graphene coating prepared by the preparation method according to claim 8.
10. Use of the aluminum oxide / graphene coating according to claim 9 in large mechanical parts.