Anti-slip stain-resistant ceramic tile and preparation method thereof
By forming anti-slip powder with a micro-convex structure on the surface of the tiles, the problem of anti-fouling agent reducing the anti-slip coefficient is solved, and the anti-slip performance and safety of the tiles are improved.
Patent Information
- Application Number
- CN202410831702.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, when applying antifouling agent on the surface of the ceramic tile to improve the antifouling ability, the anti-slip coefficient of the ceramic tile decreases, increasing the safety hazards of falling and falling injuries.
By preparing anti-slip powder and forming anti-slip agent, a micro-convex structure is formed using polyvinyl alcohol solution and ultrasonic treatment to improve the surface roughness of the ceramic tile, combined with the molar ratio of aluminum source and dissolving agent and calcining treatment, hexagonal sheet anti-slip powder is formed. Improve anti-slip performance.
It effectively improves the anti-slip coefficient of the tiles, reduces the risk of falling and injury, while maintaining the aesthetics and stain resistance of the tiles.
Smart Images

Figure CN118894738A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic tiles, and in particular to a non-slip and stain-resistant ceramic tile and a preparation method thereof. Background Art
[0002] Ceramic tiles are a kind of building decoration material with rich categories and exquisite patterns. They are often used for indoor and outdoor decoration, such as kitchens, bathrooms, indoor and outdoor floors, etc. The use of ceramic tiles can effectively improve the beauty of the building.
[0003] During the preparation process of ceramic tiles, pores will be generated on the surface of the tiles, which will cause dents or cracks on the surface of the tiles after polishing, thereby reducing the anti-fouling performance of the tiles. In order to improve the anti-fouling ability of the tiles, anti-fouling agents are usually coated on the surface of the tiles to fill the surface defects of the tiles.
[0004] However, after filling the surface defects with anti-fouling agents, the surface roughness of the tiles will be reduced, and even the anti-slip coefficient of the tiles will be reduced, which can easily lead to safety hazards such as falls and injuries. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a non-slip and stain-resistant ceramic tile and a preparation method thereof, aiming to solve the technical problem in the prior art that when an anti-fouling agent is coated on the surface of the ceramic tile to improve the anti-fouling ability of the ceramic tile, the anti-slip coefficient of the ceramic tile will be reduced, which may easily cause a safety hazard of falling and injury.
[0006] In order to achieve the above object, in a first aspect, the present invention provides a method for preparing anti-slip and stain-resistant tiles, comprising the following steps:
[0007] Preparing a ceramic tile embryo;
[0008] preparing a protective glaze, and coating the protective glaze on the embryo to form a protective layer;
[0009] Adding an aluminum source and a solvent into a first container, wherein the aluminum source is Al2(SO4)3·18H2O, and the solvent includes Na2SO4 and K2SO4, and after stirring and ultrasonic treatment, forming a first solution in the first container;
[0010] The first container is heated at a constant temperature, and a coagulant liquid is added into the first container to form a colloid in the first container;
[0011] The colloid material is sequentially subjected to drying treatment, first grinding treatment and roasting treatment to form anti-slip powder;
[0012] The anti-slip powder is prepared as an anti-slip agent based on a polyvinyl alcohol solution, the anti-slip agent is coated on the protective layer, and the anti-slip and stain-resistant ceramic tiles are formed after polishing.
[0013] Further, the preparation method of the coagulant aid liquid is:
[0014] Add Na2CO4 and deionized water into the second container and stir to form a coagulant solution.
[0015] Furthermore, the molar ratio of the aluminum source to the solvent is 1:3 to 1:5.
[0016] Furthermore, the molar ratio of the Na2SO4 to the K2SO4 is 1:1 to 2:1.
[0017] Furthermore, the temperature of the calcination treatment is 900° C. to 1200° C., and the time of the calcination treatment is 4 h to 6 h.
[0018] Furthermore, the step of preparing the anti-slip powder as an anti-slip agent based on the polyvinyl alcohol solution comprises:
[0019] Adding the anti-slip powder into a solvent to form an initial solution;
[0020] After the initial solution is subjected to ultrasonic treatment, alkaline silica sol and polyvinyl alcohol solution are added in sequence to form an anti-slip agent.
[0021] Furthermore, the anti-slip powder is added to the solvent at a concentration of 1% to 3%.
[0022] Furthermore, the step of preparing the protective glaze includes:
[0023] Mixing SiO2, CaCO3 and TiO2 into a mixed material, and performing a second grinding process on the mixed material to form a composite opacifier;
[0024] The composite opacifier is added into the glaze to form a protective glaze.
[0025] Furthermore, the second grinding treatment time is 0.5h to 3h.
[0026] In a second aspect, the present invention provides a non-slip and stain-resistant ceramic tile, which is prepared by the method for preparing the non-slip and stain-resistant ceramic tile as described in the first aspect above.
[0027] Compared with the prior art, the beneficial effect of the present invention lies in: by sequentially performing the drying treatment, the first grinding treatment and the calcining treatment on the colloid formed by mixing the aluminum source and the solvent, the anti-slip powder can be in the form of hexagonal flakes with uniformly distributed particle sizes due to the inhibitory effect of the solvent on surface growth, and then through the film-forming effect of the polyvinyl alcohol solution, during the polishing treatment, the anti-slip agent formed by the hexagonal flakes of the anti-slip powder forms a micro-convex structure on the surface of the tile, which effectively improves the surface roughness of the tile, improves the anti-slip coefficient, and reduces the risk of falling and injury. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a flow chart of the method for preparing the anti-slip and stain-resistant ceramic tile in Example 4 of the present invention;
[0029] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0031] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0033] See also Figure 1 In a first aspect, embodiment 1 of the present invention provides a method for preparing a non-slip and stain-resistant tile, comprising the following steps:
[0034] S10: preparing a ceramic tile embryo;
[0035] Specifically, different raw materials are mixed according to a preset ratio, and then subjected to milling, pressing and drying processes to form the embryo body.
[0036] S20: preparing a protective glaze, and coating the protective glaze on the embryo to form a protective layer;
[0037] The protective layer is used to improve the aesthetics of the ceramic tile and to enhance its stain resistance.
[0038] The step S20 comprises:
[0039] S210: mixing SiO2, CaCO3 and TiO2 into a mixed material, and performing a second grinding process on the mixed material to form a composite opacifier;
[0040] S220: adding the composite opacifier into the glaze to form a protective glaze;
[0041] In the traditional preparation process, TiO2 is directly used as an opacifier to prepare the protective glaze. TiO2 will combine with CaO and SiO2 in the glaze to form titanite to form an opaque phase, but a small amount of unreacted TiO2 is easily converted into a rutile phase with a non-stoichiometric ratio and coarse particles, which will cause the surface of the tile to turn yellow, thereby affecting the appearance. In this embodiment, the composite opacifier is SiO2-CaCO3-TiO2.
[0042] Through the chemical combination of the SiO2 and the CaCO3 with the TiO2, the reaction of the TiO2 into the sphene phase is induced and promoted during the preparation of the protective glaze, thereby increasing the reaction degree of the TiO2, hindering its transformation into the rutile phase, reducing the possibility of subsequent yellowing of the surface of the ceramic tile, and improving the aesthetics of the prepared ceramic tile.
[0043] In this embodiment, the second grinding treatment time is 2 hours. The glaze is obtained by grinding and slurrying a base material group, wherein the base material group includes feldspar, quartz, talc and kaolin.
[0044] S30: adding an aluminum source and a solvent into a first container, wherein the aluminum source is Al2(SO4)3·18H2O, and the solvent includes Na2SO4 and K2SO4, and after stirring and ultrasonic treatment, forming a first solution in the first container;
[0045] The solvent comprising the Na2SO4 and the K2SO4 has a lower melting point and a stronger dissolving ability. After the solvent is transformed into a liquid phase, the aluminum source is dissolved into [Al(OH6)] -3 The octahedral growth units are continuously superimposed to form two-, three- and six-dimensional growth units. During the superposition process, prisms and hexagonal columns are exposed, thus forming a hexagonal sheet structure.
[0046] Preferably, the molar ratio of the aluminum source to the solvent is 1:3-1:5, and the molar ratio of the Na2SO4 to the K2SO4 is 1:1-2:1. In this embodiment, the molar ratio of the aluminum source to the solvent is 1:4, and the molar ratio of the Na2SO4 to the K2SO4 is 1.5:1.
[0047] S40: heating the first container at a constant temperature, and adding a coagulant liquid into the first container to form a colloid in the first container.
[0048] Preferably, the constant temperature heating temperature is 60° C. to 80° C. In this embodiment, the constant temperature heating temperature is 70° C. Specifically, Na2CO4 and deionized water are added to the second container and stirred to form a coagulant liquid. After the coagulant liquid is added to the first container, the first container is stirred to form the colloid.
[0049] S50: performing a drying process, a first grinding process and a baking process on the colloid material in sequence to form an anti-slip powder.
[0050] Preferably, the drying temperature is 90°C to 110°C, and the drying time is 10h to 14h. In this embodiment, the drying temperature is 100°C, and the drying time is 12h. The calcination temperature is 1100°C, and the calcination time is 5h.
[0051] S60: preparing an anti-slip agent from the anti-slip powder based on a polyvinyl alcohol solution, coating the anti-slip agent on the protective layer, and forming an anti-slip and stain-resistant tile after polishing;
[0052] The step S60 comprises:
[0053] S610: adding the anti-slip powder into a solvent to form an initial solution;
[0054] The anti-slip powder is added to the solvent at a concentration of 2%.
[0055] S620: After ultrasonic treatment of the initial solution, silica sol and polyvinyl alcohol solution are added in sequence to form an anti-slip agent.
[0056] By sequentially performing the drying treatment, the first grinding treatment and the calcining treatment on the colloid formed by mixing the aluminum source and the solvent, the anti-slip powder can be in the form of hexagonal flakes with uniformly distributed particle sizes due to the inhibitory effect of the solvent on surface growth, and then through the film-forming effect of the polyvinyl alcohol solution, during the polishing treatment, the anti-slip agent formed by the hexagonal flakes of the anti-slip powder forms a micro-convex structure on the surface of the tile, which effectively improves the surface roughness of the tile, increases the anti-slip coefficient, and reduces the risk of falling and injury.
[0057] Embodiment 2 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0058] The second grinding treatment time is 0.5h.
[0059] Embodiment 3 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0060] The second grinding treatment time is 3 hours.
[0061] Comparative Example 1 of the present invention provides a method for preparing a non-slip and stain-resistant tile, which is different from the method for preparing a non-slip and stain-resistant tile described in Example 1 in that:
[0062] The second grinding treatment is not performed, that is, SiO2, CaCO3 and TiO2 are directly added to the glaze.
[0063] Comparative Example 2 of the present invention provides a method for preparing a non-slip and stain-resistant tile, which is different from the method for preparing a non-slip and stain-resistant tile described in Example 1 in that:
[0064] TiO2 is added to the glaze. That is, the protective glaze is prepared in a traditional manner in this comparative example.
[0065] The anti-slip and stain-resistant ceramic tiles were prepared by the preparation methods of the anti-slip and stain-resistant ceramic tiles described in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2, respectively, and the whiteness of the prepared anti-slip and stain-resistant ceramic tiles was tested. The test results are shown in the following table:
[0066]
[0067] It can be seen from the above table that the chromaticity values L * The difference is not much, that is, the brightness of different anti-slip and stain-resistant tiles is not much different, but the composite emulsifier with a SiO2-CaCO3-TiO2 composite structure formed after grinding can significantly improve the whiteness of anti-slip and stain-resistant tiles.
[0068] Embodiment 4 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0069] The calcination temperature is 900°C.
[0070] Embodiment 5 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0071] The calcination temperature is 1200°C.
[0072] Embodiment 6 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0073] The calcination time is 4 hours.
[0074] Embodiment 7 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0075] The calcination time is 6 hours.
[0076] Embodiment 8 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0077] The anti-slip powder is added to the solvent at a concentration of 1%.
[0078] Embodiment 9 of the present invention provides a method for preparing a non-slip and stain-resistant ceramic tile, which is different from the method for preparing a non-slip and stain-resistant ceramic tile described in Embodiment 1 in that:
[0079] The anti-slip powder is added to the solvent at a concentration of 3%.
[0080] Comparative Example 3 of the present invention provides a method for preparing a non-slip and stain-resistant tile, which is different from the method for preparing a non-slip and stain-resistant tile described in Example 1 in that:
[0081] The calcination temperature is 600°C.
[0082] Comparative Example 4 of the present invention provides a method for preparing a non-slip and stain-resistant tile, which is different from the method for preparing a non-slip and stain-resistant tile described in Example 1 in that:
[0083] The calcination time is 2 hours.
[0084] Comparative Example 5 of the present invention provides a method for preparing a non-slip and stain-resistant tile, which is different from the method for preparing a non-slip and stain-resistant tile described in Example 1 in that:
[0085] The anti-slip powder is added to the solvent at a concentration of 0.5%.
[0086] The anti-skid and stain-resistant ceramic tiles were prepared by the methods for preparing the anti-skid and stain-resistant ceramic tiles described in Example 1, Example 4 to Example 9 and Comparative Examples 3 to Comparative Examples 5 of the present invention, respectively, and the wet anti-skid coefficients were tested. The test results are shown in the following table:
[0087]
[0088] It can be seen from the above table that by controlling the preparation parameters of the anti-slip agent in this application, it can be ensured that the prepared anti-slip agent, when covered on ceramic tiles, reaches a standard wet anti-slip coefficient of 0.5 or above, thereby effectively improving the anti-slip effect of the ceramic tiles.
[0089] The second aspect of the present application provides a non-slip and stain-resistant ceramic tile, which is prepared by the preparation method of the non-slip and stain-resistant ceramic tile described in the first aspect above.
[0090] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0091] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing anti-skid and stain-resistant tiles, characterized in that: The following steps are involved: Preparing a ceramic tile embryo; preparing a protective glaze, and coating the protective glaze on the embryo to form a protective layer; Adding an aluminum source and a solvent into a first container, wherein the aluminum source is Al2(SO4)3·18H2O, and the solvent includes Na2SO4 and K2SO4, and after stirring and ultrasonic treatment, forming a first solution in the first container; The first container is heated at a constant temperature, and a coagulant liquid is added into the first container to form a colloid in the first container; The colloid material is sequentially subjected to drying treatment, first grinding treatment and roasting treatment to form anti-slip powder; The anti-slip powder is prepared as an anti-slip agent based on a polyvinyl alcohol solution, the anti-slip agent is coated on the protective layer, and the anti-slip and stain-resistant ceramic tiles are formed after polishing.
2. The method for preparing the anti-slip and stain-resistant ceramic tile according to claim 1, characterized in that: The preparation method of the coagulant aid liquid is: Add Na2CO4 and deionized water into the second container and stir to form a coagulant solution.
3. The method for preparing the anti-slip and stain-resistant ceramic tile according to claim 1, characterized in that: The molar ratio of the aluminum source to the solvent is 1:3 to 1:
5.
4. The method for preparing the anti-slip and stain-resistant ceramic tile according to claim 1, characterized in that: The molar ratio of the Na2SO4 to the K2SO4 is 1:1 to 2:
1.
5. The method for preparing the anti-skid and stain-resistant ceramic tile according to claim 1, characterized in that: The temperature of the calcination treatment is 900° C. to 1200° C., and the time of the calcination treatment is 4 h to 6 h.
6. The method for preparing the anti-skid and stain-resistant ceramic tile according to claim 1, characterized in that: The step of preparing the anti-slip powder as an anti-slip agent based on the polyvinyl alcohol solution comprises: Adding the anti-slip powder into a solvent to form an initial solution; After the initial solution is subjected to ultrasonic treatment, silica sol and polyvinyl alcohol solution are added in sequence to form an anti-slip agent.
7. The method for preparing the anti-skid and stain-resistant ceramic tile according to claim 6, characterized in that: The anti-slip powder is added to the solvent in a concentration of 1% to 3%.
8. The method for preparing the anti-skid and stain-resistant ceramic tile according to claim 1, characterized in that: The steps of preparing the protective glaze include: Mixing SiO2, CaCO3 and TiO2 into a mixed material, and performing a second grinding process on the mixed material to form a composite opacifier; The composite opacifier is added into the glaze to form a protective glaze.
9. The method for preparing the anti-skid and stain-resistant ceramic tile according to claim 1, characterized in that: The second grinding treatment time is 0.5h to 3h.
10. A non-slip and stain-resistant tile, characterized in that: The anti-slip and stain-resistant ceramic tile is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Titanite type compound emulsion and prepn. thereof
CN1045963A
SiO2-CaCO3-TiO2 composite ceramic opacifier based on ordered interface bonding and preparation method thereof
CN113860728A
Anti-slip protective glaze, anti-slip stain-resistant ceramic tile and preparation method of anti-slip stain-resistant ceramic tile
CN116282921A
Anti-skid wear-resistant ceramic tile with island-shaped structure and preparation method of anti-skid wear-resistant ceramic tile
CN116986925A
Anti-slip protective glaze, anti-slip ceramic tile and preparation method of anti-slip ceramic tile
CN117326887A
Cited By
Preparation method of anti-skid and antibacterial ceramic tile and anti-skid and antibacterial ceramic tile