Preparation method of croscarmellose sodium

By using commercially available hydrochloric acid as an acidifier and catalyst, the one-pot method is used to prepare croscarmellose sodium, which solves the problems of high production costs and many impurities of the product, achieves cost reduction and quality improvement, and meets the medical auxiliary materials standard.

CN118894947APending Publication Date: 2024-11-05JIANGSU XIDIAN PHARM EXCIPIENTS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411324458.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the prior art, the production cost of croscarmellose sodium is high and the product is impurities, which can cause problems such as risk of diethyl ether side reaction and inorganic salts that cannot be recovered.

Method used

Using commercially available hydrochloric acid as acidifier and catalyst, croscarmellose sodium is prepared by a one-pot method to avoid the occurrence of diethyl ether side reaction, simplify the operation steps, and slurry with ethanol aqueous solution after temperature control reaction and filtration to reduce production and the generated sodium chloride is recovered.

Benefits of technology

It effectively reduces production costs, avoids the generation of impurities, simplifies the operation steps, and meets the quality standards of pharmaceutical excipients. The water absorption expansion rate and disintegration time limit of croscarmellose sodium are better than those of the comparison samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of cross-linked sodium carboxymethyl cellulose, and relates to the technical field of pharmaceutical adjuvant production processes, and the preparation method comprises the following steps: mixing sodium carboxymethyl cellulose and an ethanol aqueous solution, stirring, dropwise adding hydrochloric acid, and carrying out temperature control reaction; adding a sodium carbonate aqueous solution for continuous reaction; after the reaction is finished, discharging and filtering; taking a filter cake, adding an ethanol water solution, pulping, filtering and drying to obtain the croscarmellose sodium. The cross-linked sodium carboxymethyl cellulose is prepared by using the commercially available hydrochloric acid as the acidifying agent and the catalyst and adopting the one-pot method, so that compared with the prior art, the side reaction of diethyl ether generation is avoided, the operation steps are reduced, and the production cost can be effectively reduced; meanwhile, only one single industrial inorganic salt sodium chloride is generated in the whole preparation process, and can be recycled and sold to generate additional value, so that the production cost is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pharmaceutical excipient production technology, in particular to a method for preparing cross-linked sodium carboxymethyl cellulose. Background Art

[0002] Crosslinked carboxymethyl cellulose sodium can be used as a disintegrant for tablets, capsules and granules in oral preparations due to its good compressibility and strong disintegration ability. It achieves the disintegration effect by capillary and swelling action. Whether crosslinked carboxymethyl cellulose sodium is added internally or externally, the brittleness of the tablet is not affected, and the disintegration time and release effect of the tablets made with it will not change over time. Due to its excellent disintegration performance, it is synthesized into four super disintegrants with crosslinked povidone, crosslinked carboxymethyl starch sodium and low-substituted hydroxypropyl cellulose.

[0003] At present, there are generally two methods for preparing cross-linked sodium carboxymethyl cellulose: one is to disperse sodium carboxymethyl cellulose in a solvent and then cross-link it under the action of a cross-linking agent; the other is to self-cross-link sodium carboxymethyl cellulose at high temperature or dissolve it in a certain solvent.

[0004] Patent CN 103059321 A discloses a method for preparing cross-linked sodium carboxymethyl cellulose using epichlorohydrin as a cross-linking agent under alkaline conditions. Although this method has many advantages such as mild reaction conditions, controllable cross-linking degree, mild reaction solvent, no organic solvent residue after the reaction, and cross-linking reaction under alkaline conditions can avoid hydrolysis of sodium carboxymethyl cellulose, epichlorohydrin is a Class 2A carcinogen and there are hidden dangers in using it as a pharmaceutical excipient.

[0005] Patent CN 113631583 A discloses a method for preparing cross-linked sodium carboxymethyl cellulose using a diglycidyl ether compound as a cross-linking agent. This preparation method has the advantages of higher safety and being more suitable for pharmaceutical excipients; a wide variety of cross-linking agents can be selected, and even multiple cross-linking agents can be added at the same time; however, due to the high price of this type of cross-linking agent, the cost is difficult to control during commercial production, and it is difficult to promote to industrial production.

[0006] Patent CN 113480669 A discloses a method for preparing cross-linked sodium carboxymethyl cellulose using concentrated sulfuric acid as an acidifier and catalyst. This preparation method does not require the addition of an additional cross-linking agent, thereby avoiding the subsequent problem of removing the cross-linking agent. Compared with the preparation of cross-linked sodium carboxymethyl cellulose by adding a cross-linking agent, this process is more suitable for industrial production. However, when concentrated sulfuric acid is used as an acidifier and a catalyst, there is a risk of generating ether as a side reaction when the concentrated sulfuric acid is added dropwise to an ethanol-water system. In this process, the cross-linking reaction and neutralization are carried out in two steps, which is relatively time-consuming in industrial production. Moreover, this process produces a variety of different inorganic salts during the preparation process, and the inorganic salts cannot be recovered to reduce costs.

[0007] Therefore, we propose a preparation method of cross-linked sodium carboxymethyl cellulose to solve the problems of high production cost and high product impurities in the prior art. Summary of the invention

[0008] The object of the present invention is to provide a method for preparing cross-linked sodium carboxymethyl cellulose to solve the problems raised in the prior art.

[0009] To achieve the above object, the present invention provides the following technical solution: a method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps: S1: mixing sodium carboxymethyl cellulose and ethanol aqueous solution, stirring to obtain a mixed slurry; S2: adding hydrochloric acid dropwise to the mixed slurry and reacting under controlled temperature; S3: After the reaction is completed, add sodium carbonate aqueous solution and control the temperature to react; S4: After the reaction is completed, discharge the material and filter; take the filter cake, add ethanol aqueous solution to pulp, filter, and dry to obtain cross-linked sodium carboxymethyl cellulose.

[0010] Furthermore, in S1, the mass ratio of sodium carboxymethyl cellulose to ethanol aqueous solution is 1:(1-20).

[0011] Furthermore, in S1, the mass fraction of the ethanol aqueous solution is 50% to 100%.

[0012] Furthermore, in S1, the temperature of the mixed slurry is -10 to 70°C.

[0013] Furthermore, the molar ratio of sodium carboxymethyl cellulose to hydrochloric acid is 1:(0.5-10).

[0014] Furthermore, in S2, hydrochloric acid is added in the form of a 12 mol / L solution, and the dropping speed is 3 to 4 drops / s.

[0015] Furthermore, in S3, the mass concentration of the sodium carbonate aqueous solution is 0.1% to 33.2%.

[0016] Furthermore, in S4, the mass fraction of the ethanol aqueous solution is 10% to 100%.

[0017] Furthermore, in S2, the process conditions of the temperature-controlled reaction are: temperature: 40-90°C, reaction time: 0.5-24h.

[0018] Furthermore, in S3, the process conditions of the temperature-controlled reaction are: temperature: -10 to 70°C, reaction time: 0.5 to 24 hours.

[0019] Furthermore, in S4, the beating time is 0.05h to 24h.

[0020] Compared with the prior art, the present invention has the following beneficial effects: The invention uses commercially available hydrochloric acid as an acidulant and a catalyst and adopts a one-pot method to prepare cross-linked sodium carboxymethyl cellulose. Compared with the existing process, the occurrence of a side reaction of generating ether is avoided, the operation steps are reduced, and the production cost can be effectively reduced. Meanwhile, the process of the invention only produces a single industrial inorganic salt, sodium chloride, in the whole preparation process, which can be recycled and sold to generate additional added value, thereby further reducing the production cost. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The following specific implementation method is a laboratory test and can be scaled up in equal proportions; Example 1: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps: S1: Add 50g of raw material sodium carboxymethyl cellulose and 500g of ethanol into a flask, stir and disperse evenly to obtain a mixed slurry, and control the temperature to 5°C; S2: 16.5 g of 12 mol / L hydrochloric acid was added dropwise to the obtained mixed slurry, and the temperature was controlled to 5°C during the process. After the addition was completed, the mixture was stirred for 15 min, and the temperature was raised to 85°C for reaction for 12 h. The addition rate was 3 drops / s. S3: After the reaction is completed, the temperature is lowered to 65°C, 250 g of 0.5% sodium carbonate aqueous solution is added to the mixed slurry, and the mixture is stirred for reaction for 0.5 h; S4: After the reaction is completed, filter, add the filter cake to 160g of ethanol and beat for 5min, filter, dry the filter cake to obtain 48.1g of dry material, and grind it.

[0023] Embodiment 2: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps: S1, add 50g raw material sodium carboxymethyl cellulose and 300g 90% ethanol water into a flask, stir and disperse evenly to obtain a mixed slurry, and control the temperature to 30°C; S2. Add 35 g of 12 mol / L hydrochloric acid to the obtained mixed slurry, control the temperature to 0°C during the process, stir for 15 min after the addition is completed, raise the temperature to 65°C, stir and react for 12 h; the drop rate is 3 drops / s; S3. After the reaction is completed, the temperature is lowered to 30°C, 250 g of 0.5% sodium carbonate aqueous solution is added to the mixed slurry, and the mixture is stirred for 12 h. S4. After the reaction is completed, filter, add the filter cake to 500 g of ethanol and beat for 12 h, filter, dry the filter cake to obtain 48.5 g of dry material, and grind it.

[0024] Example 3: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps: S1, add 50g raw material sodium carboxymethyl cellulose and 800g 80% ethanol water into a flask, stir and disperse evenly to obtain a mixed slurry, and control the temperature to -10°C; S2. Add 50 g of 12 mol / L hydrochloric acid to the obtained mixed slurry, control the temperature to -10°C during the process, stir for 15 min after the addition, raise the temperature to 40°C and react for 0.5 h; the addition speed is 3 drops / s; S3. After the reaction is completed, the temperature is lowered to -10°C, 300 g of 20% sodium carbonate aqueous solution is added to the mixed slurry, and the mixture is stirred for 0.5 h. S4. After the reaction is completed, filter, add the filter cake to 100g of ethanol and beat for 0.05h, filter, dry the filter cake to obtain 47.5g of dry material, and grind it.

[0025] Example 4: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps: S1, add 50g raw material sodium carboxymethyl cellulose and 300g 90% ethanol water into a flask, stir and disperse evenly to obtain a mixed slurry, and control the temperature to 70°C; S2, add 35g of 12mol / L hydrochloric acid to the obtained mixed slurry, control the temperature to 10°C during the process, stir for 15min after the addition, raise the temperature to 90°C and stir to react for 24h; the dropping speed is 4 drops / s; S3. After the reaction is completed, the temperature is lowered to 70°C, 250 g of 0.5% sodium carbonate aqueous solution is added to the mixed slurry, and the mixture is stirred for reaction for 24 h; S4. After the reaction is completed, filter, add the filter cake to 500 g of ethanol and beat for 24 h, filter, dry the filter cake to obtain 48.5 g of dry material, and grind it.

[0026] Comparative Example 1: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps in sequence: S1. Add 500 g of 90% ethanol water into a flask, start stirring, then add 50 g of sodium carboxymethyl cellulose, and stir to make it evenly dispersed; S2, adding 15 g of concentrated sulfuric acid with a mass fraction of 98% to the sodium carboxymethyl cellulose dispersion, then heating to 65° C., stirring and reacting at 60° C. for 6 h to obtain a cross-linked sodium carboxymethyl cellulose suspension; S3, cooling the cross-linked sodium carboxymethyl cellulose suspension in step S2 to 45° C. and filtering; S4, add the filtered cake into 500g of 20% ethanol water, slowly add saturated sodium acetate solution, adjust the pH to near neutral, and react and wash at 45°C for 1h; S5, filtering the cross-linked sodium carboxymethyl cellulose suspension obtained in step S4, adding the filter cake obtained by filtration into 70% ethanol water for pulping and washing for 1 hour, then filtering again and repeating the washing once, drying the filter cake and crushing it.

[0027] Comparative Example 2: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps in sequence: S1. Add 500 g of 90% ethanol water into a flask, start stirring, then add 50 g of sodium carboxymethyl cellulose, and stir to make it evenly dispersed; S2, adding 30 g of concentrated sulfuric acid with a mass fraction of 98% to the sodium carboxymethyl cellulose dispersion, then heating to 70° C., stirring and reacting at 65° C. for 6 h to obtain a cross-linked sodium carboxymethyl cellulose suspension; S3, cooling the cross-linked sodium carboxymethyl cellulose suspension in step S2 to 45° C. and filtering; S4, add the filtered cake into 500g 20% ​​ethanol water, slowly add saturated sodium acetate solution, adjust the pH to near neutral, and react and wash at 65°C for 1h; S5, filtering the cross-linked sodium carboxymethyl cellulose suspension obtained in step S4, adding the filter cake obtained by filtration into 70% ethanol water for pulping and washing for 1 hour, then filtering again and repeating the washing once, drying the filter cake and crushing it.

[0028] Comparative Example 3: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps in sequence: S1. Add 500 g of 90% ethanol water into a flask, start stirring, then add 50 g of sodium carboxymethyl cellulose, and stir to make it evenly dispersed; S2, adding 15 g of concentrated sulfuric acid with a mass fraction of 98% to the sodium carboxymethyl cellulose dispersion, then heating to 65° C. and reacting for 6 hours to obtain a cross-linked sodium carboxymethyl cellulose suspension; S3, cooling to 45°C and filtering; S4. Add the filtered cake into 500 g of 20% ethanol water, stir evenly, then add 48 g of saturated sodium acetate solution, pH = 5.5, and react at 65°C for 1 hour.

[0029] S5, filtering, adding the filter cake to 500g 70% ethanol water and washing for 1h, then filtering again and repeating the washing once, drying the filter cake and crushing it.

[0030] Comparative Example 4: A method for preparing cross-linked sodium carboxymethyl cellulose, comprising the following steps in sequence: S1. Add 1 g of sodium carboxymethyl cellulose to 10 mL of anhydrous ethanol to obtain a suspension; S2, adding 1 mL of 98% sulfuric acid into 15 mL of ethanol to obtain a sulfuric acid ethanol solution; S3, mixing the sulfuric acid ethanol solution obtained in S2 with the suspension in S1, heating, stirring continuously for 60 min, raising the temperature to 70° C., maintaining for 7 h, to obtain a mixture; S4, centrifugally filter the mixture obtained in S3, add 10 mL of water to the filter cake, stir and centrifuge, add anhydrous ethanol and stir and wash for 10 min, centrifuge and filter to obtain a filter cake; S5. Add 1 mL of 25% sodium bicarbonate solution to the filtered material obtained in S4, put it into a kneading mixer, mix for 20 minutes, take it out, place it in 15 mL of anhydrous ethanol, stir and react for 10 minutes, centrifuge and filter it, vacuum dry it at 100°C for 5 hours, crush it, pass it through a 200-mesh sieve, and obtain cross-linked sodium carboxymethyl cellulose; the centrifugal process conditions are: speed: 4000 r / min, time: 10 min.

[0031] experiment: Water absorption expansion rate experiment: Take the cross-linked sodium carboxymethyl cellulose prepared in Examples 1 to 4 and Comparative Examples 1 to 4, and test its water absorption expansion rate. Place the device in a constant temperature water bath at 37°C. Before starting the test, fill the pipette with water so that the liquid level of the pipette is at the same level as the filter surface of the funnel sand core; weigh 300 mg of cross-linked sodium carboxymethyl cellulose, quickly pour it into the funnel and start timing, and record the scale of the water level in the pipette at different times; the water absorption of the cross-linked sodium carboxymethyl cellulose is the volume of water reduction; Water absorption expansion rate (W) = Vρ / m, where V is the volume of the absorbed liquid, ρ is the density of the absorbed liquid, and m is the actual amount of sodium carboxymethyl cellulose weighed; Degree of substitution, sodium chloride, and sodium glycolate content detection: The degree of substitution and sodium chloride content of the cross-linked sodium carboxymethyl cellulose prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were detected according to the method specified in the "Chinese Pharmacopoeia 2020 Edition"; Disintegration time test: According to the Chinese Pharmacopoeia, the disintegration time test of the prepared cross-linked carboxymethyl cellulose sodium was carried out using the hanging basket method;

[0032] According to the data in the above table, we can clearly draw the following conclusions: The cross-linked sodium carboxymethyl cellulose prepared in Examples 1 to 4 is compared with the cross-linked sodium carboxymethyl cellulose prepared in Comparative Examples 1 to 4. The test results show that: Compared with Comparative Example 1, the cross-linked sodium carboxymethyl cellulose prepared in Examples 1 to 4 has better water absorption swelling rate, degree of substitution, shorter disintegration time, and less content of sodium chloride and sodium glycolate. It can be seen that the preparation method of the present invention has the advantages of mild conditions, simple operation steps, and no impurities introduced by cross-linking. While the cross-linked sodium carboxymethyl cellulose prepared meets the requirements of the quality standards of pharmaceutical excipients, the production cost is reduced.

[0033] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing cross-linked sodium carboxymethyl cellulose, characterized in that: The following steps are involved: S1: mixing sodium carboxymethyl cellulose and ethanol aqueous solution, stirring to obtain a mixed slurry; S2: adding hydrochloric acid dropwise to the mixed slurry and reacting under controlled temperature; S3: After the reaction is completed, add sodium carbonate aqueous solution and control the temperature to react; S4: After the reaction is completed, discharge the material and filter; take the filter cake, add ethanol aqueous solution to pulp, filter, and dry to obtain cross-linked sodium carboxymethyl cellulose.

2. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S1, the mass ratio of sodium carboxymethyl cellulose to ethanol aqueous solution is 1:(1-20).

3. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S1, the mass fraction of the ethanol aqueous solution is 50% to 100%.

4. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S1, the temperature of the mixed slurry is -10 to 70°C.

5. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: The molar ratio of sodium carboxymethyl cellulose and hydrochloric acid is 1: (0.5-10).

6. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 5, characterized in that: In S2, hydrochloric acid is added in the form of a 12 mol / L solution at a dropping speed of 3 to 4 drops / s.

7. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S3, the mass concentration of the sodium carbonate aqueous solution is 0.1% to 33.2%.

8. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S4, the mass fraction of the ethanol aqueous solution is 10% to 100%.

9. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S2, the process conditions of the temperature-controlled reaction are: temperature: 40-90°C, reaction time: 0.5-24h.

10. The method for preparing cross-linked sodium carboxymethyl cellulose according to claim 1, characterized in that: In S3, the process conditions of the temperature-controlled reaction are: temperature: -10 to 70°C, reaction time: 0.5 to 24 hours.

Citation Information

Cited By

  • Preparation method and application of cross-linked carboxymethyl cellulose

    CN120647782A