Polyoxyalkylene ether polyester polyol, preparation method thereof and high-flame-retardant rigid polyurethane foam

Through the combination of polyoxyalkylene ether polyester polyol and isocyanate, the problems of poor flame retardant performance and stability of rigid polyurethane foam are solved, and the polyoxyalkylene ether polyester foam with low viscosity, stability and high flame retardant performance are achieved. Suitable for the production of B1 grade flame retardant foam.

CN118894982APending Publication Date: 2024-11-05WANHUA CHEMYANTAI RONGWEI POLYURETHANE CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411143247.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing rigid polyurethane foam has poor flame retardant properties, and the commonly used aromatic polyester polyols have a large viscosity and are easy to crystallize, and have a short storage time, making it difficult to meet the requirements of high flame retardant and stability.

Method used

Polyoxyalkylene ether polyester polyol, which has a content of 5 to 30 wt%, polyoxyalkylene ether, 20 to 40 wt%, and polyhydric acid of 38 to 50 wt%, were prepared by one pot method to obtain low viscosity and stability. Good polyoxyalkylene ether polyester polyols and combined with isocyanate to prepare highly flame retardant rigid polyurethane foam.

Benefits of technology

The low viscosity, stability and high flame retardant properties of polyoxyalkylene ether polyester polyol are achieved. The prepared rigid polyurethane foam has good low smoke and high flame retardant properties, and is suitable for B1 grade flame retardant foam, which shortens the Reaction time and increase production capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001517780000141
    Figure BDA0005001517780000141
  • Figure BDA0005001517780000151
    Figure BDA0005001517780000151
  • Figure BDA0005001517780000152
    Figure BDA0005001517780000152
Patent Text Reader

Abstract

The invention provides polyoxyalkylene ether polyester polyol, a preparation method thereof and high-flame-retardant rigid polyurethane foam, polymeric monomers in the polyoxyalkylene ether polyester polyol comprise polyoxyalkylene ether, polyol and polybasic acid, and the content of the polyoxyalkylene ether is 5-30 wt% based on the total content of the polymeric monomers being 100 wt%. According to the polyoxyalkylene ether polyester polyol, polyester with a low hydroxyl value can have relatively low viscosity and relatively good storage stability; by adopting the polyoxyalkylene ether polyester polyol, the prepared rigid polyurethane foam shows good low-smoke property and high flame retardant property, and also has excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer materials and relates to a polyoxyalkylene ether polyester polyol and a preparation method thereof and a highly flame-retardant rigid polyurethane foam. Background Art

[0002] The flame retardancy of rigid foams based on high hydroxyl aromatic polyester polyols is better than that of foams based on polyether polyols. In the polyurethane foam industry, aromatic polyester polyols are often used to replace part or all of the polyether polyols in the formulations of polyurethane foams and polyisocyanate rigid foams. Adding some aromatic polyester polyols to the formulation of winter refrigerator components can also improve the toughness and adhesion of the foam. Phthalic anhydride polyester polyols are particularly suitable for polyisocyanurate (PIR) foams. The foam contains a large number of benzene rings, which not only improves the heat resistance of the foam, but also improves the flame retardancy of the product. Aromatic polyester polyols are widely used in the production of sandwich foam boards for construction and on-site spraying in the construction industry at home and abroad. In addition to the basic properties of polyether polyurethane rigid foams, this polyester-containing polyurethane rigid foam also has the advantages of fine foam, good toughness, excellent flame retardancy, and low price.

[0003] CN101314636A discloses a polyester synthesis method using one or more aliphatic dibasic acids and 1,2-propylene glycol as raw materials. The method solves the problem of low reaction activity of 1,2-propylene glycol and difficulty in preparing high molecular weight polymers by selecting a high-efficiency catalyst. The obtained product has excellent biodegradability and mechanical properties, can replace non-biodegradable plastics such as polyolefins, and is used in films, fibers, packaging materials, etc.

[0004] CN114599705A discloses a method for preparing high-density liquid polyester using C2-C12 polyacid and polyol as raw materials. The product can be used in lubricant compositions, improving the biodegradability and biotoxicity of the lubricant in an aqueous environment.

[0005] However, the existing patents have not yet studied the application potential of polyoxyethylene ether flame retardant polyester polyols in the field of rigid polyurethane foam. The common rigid polyurethane foams with good flame retardancy on the market mostly use aromatic polyester polyols produced from diol or triol monomers as raw materials. The products have high viscosity, easy crystallization, short storage time and poor flame retardancy. Summary of the invention

[0006] In order to solve the above technical problems, the present application provides a polyoxyalkylene ether polyester polyol and a preparation method thereof and a highly flame retardant rigid polyurethane foam. The polyoxyalkylene ether polyester polyol can be a low hydroxyl value polyester with lower viscosity and better storage stability. The rigid polyurethane foam prepared by using the polyoxyalkylene ether polyester polyol exhibits good low smoke and high flame retardant properties, and also has excellent mechanical properties.

[0007] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0008] One of the purposes of the present invention is to provide a polyoxyalkylene ether polyester polyol, wherein the polymerization monomers in the polyoxyalkylene ether polyester polyol include polyoxyalkylene ether, polyol and polyacid;

[0009] Based on the total content of the polymerized monomers being 100 wt %, the content of the polyoxyalkylene ether is 5 to 30 wt %.

[0010] The content of the polyoxyalkylene ether may be 5wt%, 10wt%, 15wt%, 20wt%, 25wt% or 30wt%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0011] As a preferred technical solution of the present invention, the molecular weight of the polyoxyalkylene ether is 200-1000, such as 200, 300, 400, 500, 600, 700, 800, 900 or 1000, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0012] Preferably, the polyoxyalkylene ether is selected from polyoxyethylene ether and / or polyoxypropylene ether.

[0013] Preferably, the polyoxyethylene ether is selected from any one of PEG200, PEG300 and PEG400, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of PEG200 and PEG300, a combination of PEG300 and PEG400, a combination of PEG200 and PEG400, or a combination of PEG200, PEG300 and PEG400, etc.

[0014] Preferably, the polyoxypropylene ether is selected from any one of PPG200, PPG300, PPG500 or PPG600, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of PPG200 and PPG300, a combination of PPG300 and PPG500, a combination of PPG500 and PPG600, a combination of PPG600 and PPG200, or a combination of PPG200, PPG300, PPG500 and PPG600, etc.

[0015] As a preferred technical solution of the present invention, based on the total content of the polymerized monomers as 100wt%, the content of the polyol is 20-40wt%, such as 20wt%, 22wt%, 25wt%, 28wt%, 30wt%, 32wt%, 35wt%, 38wt% or 40wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the polyol is selected from any one of ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerol or methylpropylene glycol, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of ethylene glycol and diethylene glycol, a combination of diethylene glycol and propylene glycol, a combination of propylene glycol and dipropylene glycol, a combination of dipropylene glycol and glycerol, a combination of glycerol and methylpropylene glycol, a combination of methylpropylene glycol and ethylene glycol, or a combination of ethylene glycol, diethylene glycol and propylene glycol, etc.

[0017] Preferably, based on the total content of the polymerized monomers as 100wt%, the content of the polyacid is 38-50wt%, such as 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt% or 50wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the polyacid is selected from any one of phthalic acid, adipic acid, glutaric acid or terephthalic acid, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of phthalic acid and benzoic acid, a combination of adipic acid and glutaric acid, a combination of glutaric acid and terephthalic acid, or a combination of phthalic acid, terephthalic acid and adipic acid, etc.

[0019] As a preferred technical solution of the present invention, the functionality of the polyoxyalkylene ether polyester polyol is 2 to 4, the hydroxyl value is 160 to 300 mgKOH / g, and the viscosity is 10000 to 50000 mPa·s at 25°C.

[0020] Wherein, the functionality can be 2, 3 or 4, the hydroxyl value can be 160mgKOH / g, 170mgKOH / g, 180mgKOH / g, 190mgKOH / g, 200mgKOH / g, 210mgKOH / g, 220mgKOH / g, 230mgKOH / g, 240mgKOH / g, 250mgKOH / g, 260mgKOH / g, 270mgKOH / g, 280mgKOH / g, 290mgKOH / g or 300mgKOH / g, etc., and the viscosity at 25°C can be 10000mPa·s, 20000mPa·s, 30000mPa·s, 40000mPa·s or 50000mPa·s, etc., but are not limited to the listed values, and other values ​​not listed within the above numerical ranges are equally applicable.

[0021] The second object of the present invention is to provide a method for preparing the polyoxyalkylene ether polyester polyol provided in the first object, the preparation method comprising:

[0022] The polyoxyalkylene ether, polyol and polyacid are mixed and then subjected to a first reaction;

[0023] A catalyst is added to carry out a second reaction to obtain the polyoxyalkylene ether polyester polyol.

[0024] As a preferred technical solution of the present invention, the temperatures of the first reaction and the second reaction are independently 200-230°C, such as 200°C, 205°C, 210°C, 215°C, 220°C, 225°C or 230°C, etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the vacuum degree of the second reaction is 50-200 Mbar, such as 50 Mbar, 60 Mbar, 80 Mbar, 100 Mbar, 120 Mbar, 150 Mbar, 180 Mbar or 200 Mbar, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] The third object of the present invention is to provide a highly flame-retardant rigid polyurethane foam. The highly flame-retardant rigid polyurethane foam comprises component A and component B. The composition of component A comprises: polyester polyol, polyether polyol, surfactant, catalyst, water, foaming agent and flame retardant. The polyester polyol comprises the polyoxyalkylene ether polyester polyol provided in the first object;

[0027] The component B is isocyanate.

[0028] As a preferred technical solution of the present invention, the mass ratio of component A to component B is 1:1.2-1.5, such as 1:1.2, 1:1.3, 1:1.4 or 1:1.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] As a preferred technical solution of the present invention, the composition of component A includes, by mass fraction: 20-65% polyester polyol, 10-60% polyether polyol, 1.0-4.0% surfactant, 1.5-5.0% catalyst, 1.5-5.0% water, 5-10% foaming agent and 10-30% flame retardant.

[0030] Among them, the mass fraction of polyester polyol can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60% or 65%, etc., the mass fraction of polyether polyol can be 10%, 20%, 30%, 40%, 50% or 60%, etc., the mass fraction of surfactant can be 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5% or 4.0%, etc., the mass fraction of catalyst can be 1.5%, 2.0%, 2.5%, 3.0%, 3.5%. , 4.0%, 4.5% or 5.0% etc., the mass fraction of water can be 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5% or 5.0% etc., the mass fraction of foaming agent can be 5%, 6%, 7%, 8%, 9% or 10% etc., the mass fraction of flame retardant can be 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28% or 30% etc., but are not limited to the listed values, and other values ​​not listed within the above numerical ranges are equally applicable.

[0031] Preferably, the polyether polyol comprises polyether polyol I and polyether polyol II.

[0032] Preferably, the mass fraction of polyether polyol I in component A is 5-50%, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the mass fraction of polyether polyol II in component A is 5-30%, such as 5%, 10%, 15%, 20%, 25% or 30%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the polyether polyol I is a sucrose-based polyether polyol having a functionality of 4 to 6, a hydroxyl value of 400 to 600 mgKOH / g, and a viscosity of 3000 to 7000 mPa·s at 25°C.

[0035] Among them, the functionality of polyether polyol I can be 4, 5 or 6, the hydroxyl value can be 400 mgKOH / g, 450 mgKOH / g, 500 mgKOH / g, 550 mgKOH / g or 600 mgKOH / g, etc., and the viscosity at 25°C can be 3000 mPa·s, 4000 mPa·s, 5000 mPa·s, 6000 mPa·s or 7000 mPa·s, etc., but it is not limited to the listed values, and other unlisted values ​​within the above numerical ranges are equally applicable.

[0036] Preferably, the polyether polyol II is a polyether polyol having a functionality of 2 to 3, a hydroxyl value of 370 to 430 mgKOH / g, and a viscosity of 300 to 400 mPa·s at 25°C.

[0037] Among them, the hydroxyl value of polyether polyol II can be 370 mgKOH / g, 380 mgKOH / g, 390 mgKOH / g, 400 mgKOH / g, 410 mgKOH / g, 420 mgKOH / g or 430 mgKOH / g, and the viscosity at 25°C can be 300 mPa·s, 310 mPa·s, 320 mPa·s, 330 mPa·s, 340 mPa·s, 350 mPa·s, 360 mPa·s, 370 mPa·s, 380 mPa·s, 390 mPa·s or 400 mPa·s, but it is not limited to the listed values, and other values ​​not listed within the above numerical ranges are equally applicable.

[0038] As a preferred technical solution of the present invention, the isocyanate is polymethylene polyphenyl isocyanate.

[0039] Preferably, the polymethylene polyphenyl isocyanate is polymethylene polyphenyl isocyanate PM-200 having a viscosity of 170 to 270 mPa·s at 25°C.

[0040] Among them, the viscosity at 25°C can be 170mPa·s, 180mPa·s, 190mPa·s, 200mPa·s, 210mPa·s, 220mPa·s, 230mPa·s, 240mPa·s, 250mPa·s, 260mPa·s or 270mPa·s, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Compared with the prior art, the present invention has at least the following beneficial effects:

[0042] (1) The present invention provides a polyoxyalkylene ether polyester polyol, which has low viscosity, is not easy to crystallize, has good storage stability, and the prepared rigid polyurethane foam has good flame retardant properties and low smoke emission, and can be used to prepare B1 grade flame retardant foam;

[0043] (2) The present invention provides a polyoxyalkylene ether polyester polyol, wherein the raw material of the polyoxyalkylene ether polyester polyol includes polyoxyalkylene ether, which reduces the loss of polyol monomers and is beneficial to shortening the overall reaction time and improving the yield and production capacity of the product compared to traditional polyester production;

[0044] (3) The present invention provides a method for preparing polyoxyalkylene ether polyester polyols, which adopts a one-pot process for preparing polyoxyalkylene ether polyester polyols, has readily available raw materials, a simple process, and a short reaction time. DETAILED DESCRIPTION

[0045] The technical solution of the present application is further described below through specific implementation methods.

[0046] A specific embodiment of the present invention provides a polyoxyalkylene ether polyester polyol, wherein the polymerization monomers in the polyoxyalkylene ether polyester polyol include polyoxyalkylene ether, polyol and polyacid, and the content of the polyoxyalkylene ether is 5 to 30 wt%.

[0047] In a specific implementation of the present invention, the polyol refers to an alcohol compound containing at least two hydroxyl groups, and the polyacid refers to a carboxylic acid compound containing at least two carboxyl groups.

[0048] In the present invention, the polymerization monomers of the polyoxyalkylene ether polyester polyol include polyoxyalkylene ethers, which can disrupt the symmetrical structure of the polyester, reduce the crystallinity between molecules, and improve turbidity. Meanwhile, the soft segments of the polyoxyalkylene ethers can reduce the viscosity of the polyester product.

[0049] A specific embodiment of the present invention provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0050] The polyoxyalkylene ether, polyol and polyacid are mixed and then subjected to a first reaction;

[0051] After the material is clarified, a catalyst is added and the temperature is lowered to carry out a second reaction to obtain the polyoxyalkylene ether polyester polyol.

[0052] In a specific implementation of the present invention, the catalyst is added after the first reaction until the material is clarified, and the clarified material means that the solid material is completely dissolved.

[0053] In a specific implementation of the present invention, the catalyst is selected from any one of tetrabutyl titanate, tetraisopropyl titanate, dibutyltin dilaurate, zinc acetate or tetrapropyl titanate or a combination of at least two thereof. The amount of the catalyst used can be 0.01 to 0.2% of the total mass of the reaction materials, preferably 0.02 to 0.15%, and more preferably 0.03 to 0.1%.

[0054] In one specific implementation of the present invention, the synthesis reaction of polyoxyalkylene ether polyester polyol can be carried out according to a set procedure;

[0055] The set-up procedure may include:

[0056] (1) heating to 160-200° C., preferably 180-200° C., introducing nitrogen, and reacting for 1-4 hours, preferably 1-2 hours;

[0057] (2) heating to 200-250° C., preferably 200-230° C., reacting for 1-8 hours, preferably 4-6 hours, adding a catalyst, and vacuuming and reducing the pressure to react for 3-12 hours, preferably 6-8 hours;

[0058] The nitrogen introduction rate is 60-100 mL / min, and the nitrogen introduction time is 4-18 hours; the vacuum degree is 50-200 Mbar.

[0059] The specific embodiment of the present invention provides a highly flame-retardant rigid polyurethane foam, the highly flame-retardant rigid polyurethane foam comprises component A and component B, the composition of the component A comprises: polyester polyol, polyether polyol, surfactant, catalyst, water, foaming agent and flame retardant, the polyester polyol comprises the above-mentioned polyoxyalkylene ether polyester polyol;

[0060] The component B is isocyanate.

[0061] In the present invention, the rigid polyurethane foam prepared by using the above-mentioned polyoxyalkylene ether polyester polyol exhibits good low smoke and high flame retardant properties. The reason is that the polyoxyalkylene ether polyester polyol contains a large amount of polyoxyalkylene ether structures. When the polyacid is phthalic acid or terephthalic acid, it also contains a large amount of benzene rings. During combustion, there will be a high carbon residue, which blocks oxygen and achieves high flame retardancy and low smoke.

[0062] In a specific implementation of the present invention, the polyester polyol includes any one of polyester polyol I, polyester polyol II, polyester polyol III, polyester polyol IV, polyester polyol V or polyester polyol VI, or a combination of at least two of them. The difference between the above six polyester polyols lies in the type and amount of polyoxyalkylene ether used.

[0063] In a specific embodiment of the present invention, component A may also include polyester polyol VII, which is prepared by polymerizing a polyol and a polyacid, such as diethylene glycol, glycerol and terephthalic acid.

[0064] In a specific implementation of the present invention, the surfactant can be any one of AK-8805, AK-158, L5440, B8642, or a combination of at least two thereof.

[0065] Further, the catalyst can be any one or at least two combinations of dimethylcyclohexylamine, dimethylbenzylamine, triethylenediamine, dimethylethanolamine, triethanolamine, pentamethyldiethylenetriamine, octanoic acid ethylenediamine, dimethyl-1,3-propylenediamine, tris(dimethylaminopropyl)hexahydrotriazine and 2,4,6-(dimethylaminomethyl)phenol. Preferably, pentamethyldiethylenetriamine, dimethylcyclohexylamine and tris(dimethylaminopropyl)hexahydrotriazine are used in combination.

[0066] Further, the foaming agent can be any one or a combination of at least two of 1,1,1,3,3-pentafluoropropane (HFC-245fa), 1,1,1,3,3-pentafluorobutane (HFC-365mfc), trans-1-chloro-3,3,3-trichloropropene (LBA), 1,1,1,4,4,4-hexafluoro-2-butene (HFO-1336mzz(Z)), cyclopentane, isopentane and n-pentane. Preferably, 1,1,3,3-pentafluorobutane (HFC-365mfc) and 1,1,3,3-pentafluoropropane (HFC-245fa) are used in combination.

[0067] Further, the flame retardant is any one or a combination of at least two of triethyl phosphate (TEP), tris(2-chloropropyl) phosphate (TCPP), dimethyl methylphosphonate (DMMP), and tris(2-chloroethyl) phosphate (TCEP). Preferably, triethyl phosphate (TEP) and tris(2-chloropropyl) phosphate (TCPP) are used in combination.

[0068] In a specific implementation of the present invention, the preparation method of rigid polyurethane rigid foam can adopt conventional methods in the art, for example, including: accurately measuring component A and component B, then mechanically stirring component A to be uniform and maintaining a constant temperature of 25°C, adding component B, stirring and mixing mechanically at high speed for a short time, and then pouring into a closed mold for foaming. Among them, conditions such as stirring rate, reaction temperature and time can be further selected by those skilled in the art according to product needs, and are not further limited here.

[0069] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0070] Example 1

[0071] This embodiment provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0072] 547.5 g of polyoxyethylene ether, 543.3 g of diethylene glycol, 75.6 g of glycerol and 722 g of terephthalic acid were put into a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200 ° C, reacted for 2 hours, and then the temperature was raised to 230 ° C, and reacted until the material was clear; 0.5 g of catalyst tetrabutyl titanate was added, and the vacuum was reduced to a vacuum degree of 150 mbar and reacted for 6 hours;

[0073] Among them, polyoxyethylene ether accounts for 31% of the total material;

[0074] The obtained polyoxyethylene ether polyester polyol I has a functionality of 2 to 3, a hydroxyl value of 190.59 mg KOH / g, a viscosity of 18000 mPa·s at 25°C, and an acid value of 1.98 mg KOH / g.

[0075] Example 2

[0076] This embodiment provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0077] 273 g of polyoxyethylene ether, 579.3 g of diethylene glycol, 75.6 g of glycerol, and 822 g of terephthalic acid were placed in a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200 ° C, and the reaction was carried out for 2 hours, and then the temperature was raised to 230 ° C, and the reaction was carried out until the material was clear; 0.5 g of catalyst tetrabutyl titanate was added, and the vacuum was reduced to a vacuum degree of 150 mbar and the reaction was carried out for 6 hours;

[0078] Among them, polyoxyethylene ether accounts for 16% of the total material;

[0079] The obtained polyoxyethylene ether polyester polyol II has a functionality of 2 to 3, a hydroxyl value of 189.61 mgKOH / g, a viscosity of 22000 mPa·s at 25°C, and an acid value of 2.45 mgKOH / g.

[0080] Example 3

[0081] This embodiment provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0082] 120 g of polyoxyethylene ether, 708.5 g of diethylene glycol, 75.6 g of glycerol, and 922 g of terephthalic acid were placed in a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200 ° C, and the reaction was carried out for 2 hours, and then the temperature was raised to 230 ° C, and the reaction was carried out until the material was clear; 0.5 g of catalyst tetrabutyl titanate was added, and the vacuum was reduced to a vacuum degree of 150 mbar and the reaction was carried out for 6 hours;

[0083] Among them, polyoxyethylene ether accounts for 7% of the total material;

[0084] The obtained polyoxyethylene ether polyester polyol III has a functionality of 2 to 3, a hydroxyl value of 190.60 mgKOH / g, a viscosity of 27000 mPa·s at 25°C, and an acid value of 2.11 mgKOH / g.

[0085] Example 4

[0086] This embodiment provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0087] 547.5 g of polyoxypropylene ether, 428.0 g of diethylene glycol, 75.6 g of glycerol, and 722 g of terephthalic acid were placed in a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200 ° C, and the reaction was carried out for 2 hours, and then the temperature was raised to 230 ° C, and the reaction was carried out until the material was clarified; 0.5 g of catalyst tetrabutyl titanate was added, and the vacuum was reduced to a vacuum degree of 150 mbar and the reaction was carried out for 6 hours;

[0088] Among them, polyoxypropylene ether accounts for 31% of the total material;

[0089] The obtained polyoxypropylene ether polyester polyol IV has a functionality of 2-3, a hydroxyl value of 190.59 mgKOH / g, a viscosity of 20000 mPa·s at 25°C, and an acid value of 1.98 mgKOH / g.

[0090] Example 5

[0091] This embodiment provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0092] 273.0 g of polyoxypropylene ether, 579.3 g of diethylene glycol, 75.6 g of glycerol, and 822 g of terephthalic acid were placed in a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200° C., the reaction was carried out for 2 hours, and the temperature was raised to 230° C., and the reaction was carried out until the material was clarified; 0.5 g of catalyst tetrabutyl titanate was added, and the pressure was reduced to a vacuum degree of 150 mbar and the reaction was carried out for 6 hours;

[0093] Among them, polyoxypropylene ether accounts for 16% of the total material;

[0094] The obtained polyoxypropylene ether polyester polyol V has a functionality of 2-3, a hydroxyl value of 189.61 mgKOH / g, a viscosity of 24000 mPa·s at 25°C, and an acid value of 2.41 mgKOH / g.

[0095] Example 6

[0096] This embodiment provides a method for preparing a polyoxyalkylene ether polyester polyol, the preparation method comprising:

[0097] 120 g of polyoxypropylene ether, 708.5 g of diethylene glycol, 75.6 g of glycerol, and 922 g of terephthalic acid were placed in a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200 ° C, and the reaction was carried out for 2 hours, and then the temperature was raised to 230 ° C, and the reaction was carried out until the material was clarified; 0.5 g of catalyst tetrabutyl titanate was added, and the vacuum was reduced to a vacuum degree of 150 mbar and the reaction was carried out for 6 hours;

[0098] Among them, polyoxyethylene ether accounts for 7% of the total material;

[0099] The obtained polyoxyethylene ether polyester polyol VI has a functionality of 2-3, a hydroxyl value of 190.60 mgKOH / g, a viscosity of 30000 mPa·s at 25°C, and an acid value of 2.1 mgKOH / g.

[0100] Example 7

[0101] 422.3 g of polyoxyethylene ether, 396.1 g of diethylene glycol, 107.3 g of ethylene glycol, and 643.3 g of phthalic anhydride were placed in a reactor, replaced with nitrogen, introduced with nitrogen at 10 mL / min, heated to 200°C, reacted for 2 hours, then heated to 230°C, reacted until the material was clear; 0.5 g of tetrabutyl titanate catalyst was added, vacuumed and depressurized to a vacuum degree of 150 mbar, and reacted for 6 hours;

[0102] Among them, polyoxyethylene ether accounts for 27% of the total material;

[0103] The obtained polyoxyethylene ether polyester polyol VII has a functionality of 2 to 3, a hydroxyl value of 190.30 mgKOH / g, a viscosity of 15000 mPa·s at 25°C, and an acid value of 1.96 mgKOH / g.

[0104] Example 8

[0105] 588.3g of polyoxyethylene ether, 144.7g of methyl propylene glycol, 320.8g of ethylene glycol, and 856.5g of adipic acid were put into a reactor, replaced with nitrogen, nitrogen was introduced at 10mL / min, the temperature was raised to 200°C, the reaction was carried out for 2 hours, and the temperature was raised to 230°C, and the reaction was carried out until the material was clear; 0.5g of catalyst tetrabutyl titanate was added, and the vacuum was reduced to a vacuum degree of 150mbar and the reaction was carried out for 6 hours;

[0106] Among them, polyoxyethylene ether accounts for 31% of the total material;

[0107] The obtained polyoxyethylene ether polyester polyol VIII has a functionality of 2-3, a hydroxyl value of 189.95 mgKOH / g, a viscosity of 13000 mPa·s at 25°C, and an acid value of 1.98 mgKOH / g.

[0108] Comparative Example

[0109] 638.2 g of diethylene glycol, 75.6 g of glycerol and 822.0 g of terephthalic acid were put into a reactor, replaced with nitrogen, nitrogen was introduced at 10 mL / min, the temperature was raised to 200°C, the reaction was carried out for 2 hours, and the temperature was raised to 230°C, and the reaction was carried out until the material was clear; 0.5 g of tetrabutyl titanate catalyst was added, the pressure was reduced to 150 mbar and the reaction was carried out for 6 hours;

[0110] The comparative example does not include polyoxyalkylene ether;

[0111] The obtained polyester polyol IX has a functionality of 2 to 3, a hydroxyl value of 190.22 mgKOH / g, a viscosity of 37000 mPa·s at 25°C, and an acid value of 2.11 mgKOH / g.

[0112] The polyoxyethylene ethers used in Examples 1-8 are PEG300 polyoxyethylene ether and PPG300 polyoxypropylene ether produced by Wanhua Chemical Group Co., Ltd., with a functionality of 2 and a hydroxyl value of 374.

[0113] Application Examples

[0114] Application Examples 1-8 respectively provide a highly flame-retardant rigid polyurethane foam, which uses the polyoxyalkylene ether polyester polyol synthesized in Examples 1-8, and the composition (mass fraction) of its component A is shown in Table 1.

[0115] Comparative Application Examples

[0116] The comparative application example provides a rigid polyurethane foam using the polyester polyol synthesized in the comparative example, and the composition (mass fraction) of component A thereof is shown in Table 1.

[0117] Among them, polyether polyol I is R4110B polyether polyol produced by Wanhua Chemical Group Co., Ltd., with a functionality of 5, a hydroxyl value of 440 mgKOH / g, and a viscosity of 3134 mPa·s at 25°C.

[0118] Polyether polyol II is A310 low-functional polyether polyol produced by Wanhua Chemical Group Co., Ltd., with a functionality of 3, a hydroxyl value of 165 mgKOH / g, and a viscosity of 100-150 mPa·s at 25°C.

[0119] The surfactants are a compound of AK-8805, AK-158 and B8642.

[0120] The catalyst is a composite of dimethylcyclohexylamine (PC8), pentamethyldiethylenetriamine (PC5) and potassium acetate.

[0121] The foaming agent is a mixture of 1,1,1,3,3-pentafluoropropane (HFC-245fa) and 1,1,1,3,3-pentafluorobutane (HFC-365mfc).

[0122] The flame retardant is a mixture of triethyl phosphate (TEP) and tri(2-chloropropyl) phosphate (TCPP).

[0123] Component B is polymethylene polyphenyl isocyanate PM-400 produced by Wanhua Chemical Group Co., Ltd., with a viscosity of 403 mPa·s at 25°C.

[0124] Table 1

[0125]

[0126]

[0127]

[0128]

[0129] Comparative Application Examples Polyester polyol IX 65 Polyether polyol Ⅰ 6 Polyether polyol Ⅱ 10 Surfactant AK-8805 0.8 Surfactant AK-158 0.5 Surfactant B8642 0.4 Catalyst PC8 0.3 Catalyst PC5 0.5 Catalyst Potassium Acetate 1.0 Blowing agent HFC-245fa 4 Blowing agent HFC-365mfc 7 TEP 9 TCPP 5 water 1.5

[0130] The above-mentioned component A was respectively molded and foamed with polymethylene polyphenyl isocyanate PM-400 at a weight ratio of 1:2 at 25°C to obtain a flame-retardant rigid polyurethane foam. The relevant properties were tested after aging at room temperature for 24 hours.

[0131] Performance testing standards and methods:

[0132] The viscosity and crystallinity (after two months of storage) of Examples 1-8 and the comparative application examples were tested, and the results are shown in Table 2.

[0133] The stability and foam performance of the combined materials of Example 1-8 and the comparative application example were tested, and the results are shown in Table 3.

[0134] Oxygen index: GB / T 2406.2-2009 is a test method for determining the minimum oxygen concentration (also known as oxygen index) required to just maintain the combustion of the sample in a mixed flow of oxygen and nitrogen.

[0135] Compression strength: GB / T 8813-2008 Determination of compression properties of rigid foam plastics.

[0136] Density: GB / T 6343-2009 rigid foam plastic density test.

[0137] Table 2

[0138] Viscosity mPa·s Crystallinity (2 months) Example 1 18000 clarify Example 2 22000 clarify Example 3 27000 Slightly turbid Example 4 20000 clarify Example 5 24000 clarify Example 6 30000 clarify Example 7 15000 clarify Example 8 13000 clarify Comparative Example 37000 turbid

[0139] Table 3

[0140]

[0141] The results of the examples show that:

[0142] 1. The introduction of polyoxyalkylene ether into polyester can reduce the viscosity of low hydroxyl value highly flame retardant polyester products, reduce the crystallinity of polyester, and increase the storage stability of polyester;

[0143] 2. The introduction of polyoxyalkylene ether polyester monomers can effectively improve the compressive strength of the combined polyether. The compressive strength of the obtained rigid polyurethane foam is higher than the common foam board strength requirement (150kPa). Compared with the rigid polyurethane foam containing aromatic polyester in the comparative example, the oxygen index is significantly improved, the flame retardant performance is good, and it can be used for the production of B1 grade rigid polyurethane flame retardant foam.

[0144] 3. Compared with Example 7 and Example 8, the terephthalic acid polyester system can effectively improve the oxygen index and the flame retardancy of the foam, and can be used for the production of B1 grade rigid polyurethane flame retardant foam.

[0145] The applicant declares that the present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A polyoxyalkylene ether polyester polyol, characterized in that: The polymerization monomers in the polyoxyalkylene ether polyester polyol include polyoxyalkylene ether, polyol and polyacid; Based on the total content of the polymerized monomers being 100 wt %, the content of the polyoxyalkylene ether is 5 to 30 wt %.

2. The polyoxyalkylene ether polyester polyol according to claim 1, characterized in that The molecular weight of the polyoxyalkylene ether is 200 to 1000; Preferably, the polyoxyalkylene ether is selected from polyoxyethylene ether and / or polyoxypropylene ether; Preferably, the polyoxyethylene ether is selected from any one or a combination of at least two of PEG200, PEG300 and PEG400; Preferably, the polyoxypropylene ether is selected from any one of PPG200, PPG300, PPG500 or PPG600, or a combination of at least two thereof.

3. The polyoxyalkylene ether polyester polyol according to claim 1 or 2, characterized in that: Based on the total content of the polymerized monomers as 100 wt %, the content of the polyol is 20 to 40 wt %; Preferably, the polyol is selected from any one or a combination of at least two of ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerol or methyl propylene glycol; Preferably, based on 100 wt% of the total content of the polymerized monomers, the content of the polyacid is 38-50 wt%; Preferably, the polyacid is selected from any one of phthalic acid, adipic acid, glutaric acid or terephthalic acid, or a combination of at least two thereof.

4. The polyoxyalkylene ether polyester polyol according to any one of claims 1 to 3, characterized in that The functionality of the polyoxyalkylene ether polyester polyol is 2-4, the hydroxyl value is 160-300 mgKOH / g, and the viscosity at 25° C. is 10000-50000 mPa·s.

5. A method for preparing the polyoxyalkylene ether polyester polyol according to any one of claims 1 to 4, characterized in that: The preparation method comprises: The polyoxyalkylene ether, polyol and polyacid are mixed and then subjected to a first reaction; A catalyst is added to carry out a second reaction to obtain the polyoxyalkylene ether polyester polyol.

6. The preparation method according to claim 5, characterized in that: The temperatures of the first reaction and the second reaction are independently 200-230°C; Preferably, the vacuum degree of the second reaction is 50-200 Mbar.

7. A highly flame-retardant rigid polyurethane foam, characterized in that: The highly flame-retardant rigid polyurethane foam comprises component A and component B, wherein the composition of component A comprises: polyester polyol, polyether polyol, surfactant, catalyst, water, foaming agent and flame retardant, and the polyester polyol comprises the polyoxyalkylene ether polyester polyol according to any one of claims 1 to 4; The component B is isocyanate.

8. The highly flame-retardant rigid polyurethane foam according to claim 7, characterized in that: The mass ratio of component A to component B is 1:1.2-1.

5.

9. The highly flame-retardant rigid polyurethane foam according to claim 7, characterized in that: The composition of component A includes, by mass percentage, 20-65% polyester polyol, 10-60% polyether polyol, 1.0-4.0% surfactant, 1.5-5.0% catalyst, 1.5-5.0% water, 5-10% foaming agent and 10-30% flame retardant; Preferably, the polyether polyol comprises polyether polyol I and polyether polyol II; Preferably, the mass fraction of polyether polyol I in component A is 5 to 50%; Preferably, the mass fraction of polyether polyol II in component A is 5 to 30%; Preferably, the polyether polyol I is a sucrose-based polyether polyol having a functionality of 4 to 6, a hydroxyl value of 400 to 600 mgKOH / g, and a viscosity of 3000 to 7000 mPa·s at 25°C; Preferably, the polyether polyol II is a polyether polyol having a functionality of 2 to 3, a hydroxyl value of 370 to 430 mgKOH / g, and a viscosity of 300 to 400 mPa·s at 25°C.

10. The highly flame-retardant rigid polyurethane foam according to claim 7, characterized in that: The isocyanate is polymethylene polyphenyl isocyanate; Preferably, the polymethylene polyphenyl isocyanate is polymethylene polyphenyl isocyanate PM-200 having a viscosity of 170 to 270 mPa·s at 25°C.

Citation Information

Patent Citations

  • Biodegradable aliphat dibasic acid 1,2-propylene glycol ester and copolyester, and preparation thereof

    CN101314636A

  • High density polyester products, compositions and uses

    CN114599705A

  • Polyether ester for adhesion of textile adhesive

    CN103044670A

  • Polyether ester type polyurethane coating material and controlled-release fertilizer prepared from same

    CN112048055A

  • Flame-retardant polyether ester polyol as well as preparation method and application thereof

    CN117986552A