MLCC release film and preparation method and application thereof

By adding spherical nanosilicon dioxide to the base film of MLCC release film and controlling its particle size, the problems of high surface roughness and insufficient dispersion uniformity in the prior art are solved, and better peelability and smoothness are achieved. Easy to stable production of MLCC capacitors.

CN118895035AActive Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310491786.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-05
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

The existing MLCC release film base film has a high surface roughness, which affects its peelability and the uniformity of the clay layer thickness. In addition, the uniformity of dispersion of inorganic fillers is insufficient, making it difficult to meet the demand for stable production.

Method used

The spherical nanosilicon dioxide is added during the esterification reaction of the polyester-based film, and the median particle size and diameter distance are limited to achieve uniform dispersion of nanosilicon dioxide in the polyester matrix, reducing surface roughness and viscosity. Improve the friction coefficient and facilitate subsequent peeling.

Benefits of technology

The surface roughness, viscosity, and friction coefficient of the MLCC release film are reduced, which improves the peelability and smoothness, making it easier to subsequently prepare chip-type multi-layer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895035A_ABST
    Figure CN118895035A_ABST
Patent Text Reader

Abstract

The invention relates to the field of polymer chemical industry, and discloses an MLCC release film and a preparation method and application thereof. The surface roughness Ra of the release film is smaller than or equal to 25 nm, the surface roughness Rq is smaller than or equal to 50 nm, and the surface roughness Rz is smaller than or equal to 293 nm. The preparation method of the MLCC release film comprises the following steps: S1, under an esterification reaction condition, carrying out a first-stage reaction on a binary acid monomer, a dihydric alcohol monomer and a catalyst to obtain a reactant I; s2, under the polycondensation reaction condition, mixing the reactant I and dispersion liquid containing spherical nano silicon dioxide, and carrying out second-stage reaction to obtain polyester for the MLCC release film base film; the median value of the particle size of the spherical nano silicon dioxide is 150 to 800 nm, and the span is 1.2 to 2.5; and S3, mixing the polyester for the base film of the MLCC release film with conventional polyester, and stretching to form the film. The surface roughness of the release film is low, the stripping requirement can be met, and subsequent application of the release film in preparation of the chip multilayer ceramic capacitor is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer chemical industry, and in particular to an MLCC release film and a preparation method and application thereof. Background Art

[0002] MLCC chip-type multilayer ceramic capacitor (Multi-Layer Ceramic Capacitors) release film is mainly used in the production of MLCC. MLCC is known as "industrial rice" because of its wide range of uses. Its main terminal applications are smart phones, laptops, automotive electronics, smart wearable devices, etc. The MLCC manufacturing process is to use polyester film as the base film, first apply a silicone coating on the surface of the base film to prepare a release film, then evenly apply liquid clay on the surface of the silicone coating, then print electrodes on the clay layer, and then stack, press, sinter and shape the clay layer with printed electrodes, and then cut and other post-processing procedures to make a chip-type multilayer ceramic capacitor.

[0003] MLCC release film is a key material for MLCC, which plays the role of supporting the clay layer. It has uniform thickness, good peelability and smoothness. It needs to ensure that it can be easily peeled off after drying without damaging the dielectric layer, so as to be used for subsequent MLCC stacking. The key material of the release film is the base film. Compared with other plastic films, polyester film has excellent dimensional stability, chemical resistance and good processability, so it is used as the base film of MLCC release film. The polyester base film needs to be added with an anti-blocking agent to play an anti-adhesion and smooth role, but the existing polyester base film will cause uneven coating after subsequent coating, which affects the peelability and smoothness of the release film, and brings adverse effects on the processing of the clay layer, especially affecting the thickness uniformity of the clay layer.

[0004] The release film base film in Chinese patent application 201911336964.2 includes a first layer, a second layer and a third layer, the third layer contains 50 grams of a third layer modified polyester base material and 50 grams of a third layer surface modified material, the third layer modified polyester base material contains 1 gram of a first copolyester and 49 grams of a third layer polyester base material. The invention introduces a copolyester for improving stiffness, and its preparation process is complicated, which increases the complexity of using the film recycled material, and the introduced inorganic filler is also added by blending, and it is difficult to ensure uniformity. Chinese patent application 201911337225.5 discloses a high-adhesion release film base film for MLCC process and its preparation method. The product of the invention includes a first layer, a second layer and a third layer. The components of the third layer coating liquid include resin, N,N-dimethylethanolamine, surfactant, defoamer, curing agent, etc. The resin forms a dense resin layer after cross-linking, which can effectively block oligomers and prevent them from entering the release layer, thereby reducing residual adhesion. A large number of organic additives are introduced in this invention. Chinese patent applications 202011063754.3, 202011014739.X, 202111585609.6, etc. also use a similar coating liquid curing method to prepare MLCC films. It is difficult to ensure the uniformity of the curing reaction through the film forming process. The MLCC release film base film disclosed in Chinese patent application 202111623727.1 has an ABA-type structure. Nano-silica particles are added to the A-layer polyester in the esterification feeding stage by an in-situ polymerization method to improve the dispersion effect. The online coating surface is provided with surface smoothness by the coating liquid on the A-layer nanoparticles and the leveling property of the coating liquid. The non-coated surface is provided with low roughness by the good dispersion of the in-situ copolymerization of nano-silica, which solves the coexistence problem of openness and smoothness. The nanoparticles used in this invention are gas-phase nano-inorganic materials with a particle size between 100-150nm. The gas-phase nano-inorganic materials are fed in the esterification stage, and the powder particle size is too small to achieve uniform dispersion.

[0005] Although there have been some improvements in the preparation of MLCC release film base films in recent years through online coating, introduction of copolyesters, blending and adding nanomaterials, etc., it still cannot meet the needs of stable MLCC production in terms of reducing roughness, using film recycling, and uniformity of inorganic filler dispersion. Summary of the invention

[0006] The purpose of the present invention is to overcome the technical problem of high roughness of the MLCC release film base film in the prior art, and to provide an MLCC release film and a preparation method and application thereof.

[0007] The inventor of the present invention unexpectedly discovered in the research that by adding spherical nano-silica to the polyester used for the MLCC release film base film during the reaction process and limiting the median particle size d (0.50) and diameter distance of the spherical nano-silica, the spherical nano-silica can be evenly dispersed in the polyester matrix, effectively reducing the surface roughness of the MLCC release film, and reducing its viscosity, so that its friction system meets the requirements, achieving anti-adhesion effect, facilitating subsequent peeling, and facilitating subsequent application in the preparation of chip-type multilayer ceramic capacitors. Moreover, the basic component of the MLCC release film is still conventional polyester, which is conducive to subsequent reuse. Based on the above findings, the present invention is proposed.

[0008] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an MLCC release film, wherein the surface roughness Ra of the release film is less than or equal to 25nm, the surface roughness Rq is less than or equal to 50nm, the surface roughness Rz is less than or equal to 293nm, and the friction coefficient is less than or equal to 0.4.

[0009] Among them, the film roughness index is tested by a roughness meter, Ra: arithmetic mean height, which represents the arithmetic mean of the absolute value of the average surface height to the plane; Rz: maximum height of the film, which represents the distance from the highest point to the lowest point on the surface; Rq: root mean square height of the film, which is equivalent to the parameter of the standard deviation of the distance to the average surface, that is, the standard deviation of the height.

[0010] According to the present invention, the dynamic friction coefficient and the static friction coefficient of the release film are both less than or equal to 0.4.

[0011] Preferably, the surface roughness Rp of the release film is less than or equal to 190 nm. Rp: maximum peak height of the film, representing the maximum value of the average height to the surface.

[0012] A second aspect of the present invention provides a method for preparing an MLCC release film, the method comprising the following steps:

[0013] S1. Under esterification reaction conditions, a dibasic acid monomer, a diol monomer and a catalyst are reacted in a first stage to obtain a reactant I;

[0014] S2. Under polycondensation reaction conditions, the reactant I and the dispersion containing spherical nano-silicon dioxide are mixed to carry out a second-stage reaction to obtain a polyester for a MLCC release film base film; the median particle size of the spherical nano-silicon dioxide is 150-800 nm, and the diameter distance is 1.2-2.5;

[0015] S3, mixing the MLCC release film base film polyester and conventional polyester and stretching the mixture into a film to obtain the MLCC release film.

[0016] A third aspect of the present invention provides the use of the above-mentioned MLCC release film or the MLCC release film prepared by the above-mentioned method in the preparation of chip-type multilayer ceramic capacitors.

[0017] A fourth aspect of the present invention provides the use of the above-mentioned MLCC release film or the MLCC release film prepared by the above-mentioned method in the preparation of smart phones, laptop computers or automobiles.

[0018] The surface roughness index Ra of the MLCC release film provided by the present invention is less than or equal to 25nm, the surface roughness Rq is less than or equal to 50nm, the surface roughness Rz is less than or equal to 293nm, the friction coefficient is less than or equal to 0.4, the surface roughness is low, the viscosity is low, the anti-adhesion effect is achieved, and the subsequent peeling is convenient, and the subsequent application in the preparation of chip-type multilayer ceramic capacitors is convenient. Moreover, the basic component of the MLCC release film is still conventional polyester, which is conducive to subsequent reuse. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a SEM image of the silicon dioxide used in Example 1;

[0020] Figure 2 is a SEM image of the silicon dioxide used in Comparative Example 3;

[0021] Figure 3 is a SEM picture of the silicon dioxide used in Comparative Example 4. DETAILED DESCRIPTION

[0022] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0023] As mentioned above, the first aspect of the present invention provides an MLCC release film, the surface roughness Ra of the release film is less than or equal to 25nm, the surface roughness Rq is less than or equal to 50nm, the surface roughness Rz is less than or equal to 293nm, and the friction coefficient is less than or equal to 0.4.

[0024] Among them, the film roughness index is tested by a roughness meter, Ra: arithmetic mean height, which represents the arithmetic mean of the absolute value of the average surface height to the plane; Rz: maximum height of the film, which represents the distance from the highest point to the lowest point on the surface; Rq: root mean square height of the film, which is equivalent to the parameter of the standard deviation of the distance to the average surface, that is, the standard deviation of the height.

[0025] According to the present invention, each surface roughness parameter is tested under white light interference conditions, and the testing instrument is a laser confocal microscope. The friction coefficient includes a dynamic friction coefficient and a static friction coefficient, and the dynamic friction coefficient and the static friction coefficient of the release film are both less than or equal to 0.4.

[0026] The MLCC release film provided by the present invention has a relatively smooth surface and low viscosity, and can achieve an anti-adhesion effect, facilitate subsequent peeling, and facilitate subsequent application in the preparation of chip-type multilayer ceramic capacitors. Moreover, the basic components of the MLCC release film are still conventional, which is conducive to subsequent reuse.

[0027] According to the present invention, preferably, the surface roughness Rp of the release film is less than or equal to 190 nm. Wherein, Rp is the maximum peak height of the film, which represents the maximum value of the average surface height to the surface.

[0028] According to the present invention, preferably, the surface roughness Ra of the release film is less than or equal to 15nm, the surface roughness Rq is less than or equal to 10nm, and the surface roughness Rz is less than or equal to 50nm. The surface of the release film limited by the above conditions is smoother. Considering that the smoothness of the release film can be further improved, preferably, the surface roughness Ra of the release film is less than or equal to 7nm, the surface roughness Rq is less than or equal to 7nm, and the surface roughness Rz is less than or equal to 46nm.

[0029] According to the present invention, preferably, the surface roughness Rp of the release film is less than or equal to 40 nm. The surface of the release film limited by the above conditions is smoother. In order to further improve the smoothness of the release film, preferably, the surface roughness Rp of the release film is less than or equal to 35 nm.

[0030] A second aspect of the present invention provides a method for preparing an MLCC release film, the method comprising the following steps:

[0031] S1. Under esterification reaction conditions, a dibasic acid monomer, a diol monomer and a catalyst are reacted in a first stage to obtain a reactant I;

[0032] S2. Under polycondensation reaction conditions, the reactant I and the dispersion containing spherical nano-silicon dioxide are mixed to carry out a second-stage reaction to obtain a polyester for an MLCC release film base film; the median particle size of the spherical nano-silicon dioxide is 150-800 nm, and the diameter distance is 1.2-2.5;

[0033] S3, mixing the MLCC release film base film polyester and conventional polyester and stretching the mixture into a film to obtain the MLCC release film.

[0034] According to the present invention, the dispersion liquid containing spherical nano-silicon dioxide can take dibasic acid monomers and / or diol monomers as dispersion solvents. Preferably, the dispersion solvent of the dispersion liquid containing spherical nano-silicon dioxide is diol monomers.

[0035] The preparation method of the present invention adds spherical nano-silica at the end of the first stage reaction and limits the median particle size d (0.50) and diameter distance of the spherical nano-silica, so as to achieve uniform dispersion of the spherical nano-silica in the polyester matrix, effectively reduce the surface roughness of the MLCC release film, and reduce its viscosity, so that its friction coefficient meets the requirements, achieve anti-adhesion effect, facilitate subsequent peeling, and facilitate subsequent application in the preparation of chip-type multilayer ceramic capacitors. The surface roughness Ra of the release film obtained by the above method is less than or equal to 25nm, the surface roughness Rq is less than or equal to 50nm, the surface roughness Rz is less than or equal to 293nm, and the friction coefficient is less than or equal to 0.4. Moreover, the basic component of the MLCC release film is still conventional polyester, which is conducive to subsequent reuse.

[0036] The release film can be a film with the above-mentioned surface roughness made of spherical nano-silica and polyester in any manner. Preferably, the release film contains polyester for MLCC release film base film and conventional polyester, and the mass ratio of the polyester for MLCC release film base film to the conventional polyester is 1:0.7-3. Preferably, the raw material components of the polyester for MLCC release film base film contain dibasic acid monomers, diol monomers, spherical nano-silica and catalysts. Spherical nano-silica is added to the raw material components of the polyester for MLCC release film base film, and the polyester for MLCC release film base film and the conventional polyester are mixed according to the above-mentioned mass ratio. The obtained release film has a high smoothness and a small friction coefficient, which meets the peeling requirements and is convenient for subsequent application in the preparation of chip-type multilayer ceramic capacitors.

[0037] In the present invention, the conventional polyester can be a commercially available common polyester for preparing MLCC release film, or a polyester prepared by a conventional method in the art. Exemplarily, the preparation method of the conventional fiber includes the following steps: ethylene glycol antimony catalyst, terephthalic acid (PTA) and ethylene glycol (EG) are mixed in a weight ratio of 1:2800-3200:1600-2000, and a conventional esterification reaction is carried out under a gauge pressure of 0.2-0.3MPa and a temperature of 200-300°C; after the esterification reaction is completed, a pre-polycondensation reaction is carried out at 260-275°C for 40-50min, and finally the polycondensation reaction temperature is controlled at 270-285°C for a final polycondensation reaction, the absolute pressure is below 100Pa, and the cumulative polycondensation time is 100-110min after the stirring current of the reactor reaches the set value, and the melt is extruded by a melt pump, pelletized, and dried to obtain a conventional polyester.

[0038] Preferably, in the release film, the content of the spherical nano-silicon dioxide is 0.1-0.6wt%, specifically 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, or any value between these values. Limiting the content of the spherical nano-silicon dioxide to the above range can further improve the surface smoothness of the prepared release film and reduce the friction coefficient. Considering that the surface roughness of the release film can be further reduced, it is further preferred that in the release film, the content of the spherical nano-silicon dioxide is 0.1-0.25wt%.

[0039] Preferably, the median particle size d(0.50) of the spherical nano-silicon dioxide is 150-800nm, specifically 150nm, 300nm, 450nm, 600nm, 750nm, 800nm, or any value between these values; the diameter distance is 1.2-2.5, specifically 1.2, 1.5, 2, 2.5, or any value between these values. The spherical nano-silicon dioxide with the above conditions can further improve the surface smoothness of the prepared release film and reduce the friction coefficient. Considering that the surface roughness of the release film can be further reduced, it is further preferred that the median particle size d(0.50) of the spherical nano-silicon dioxide is 150-400nm, and the diameter distance is 1.5-2.5.

[0040] According to the present invention, preferably, the dibasic acid monomer can be selected from at least one of terephthalic acid, isophthalic acid and adipic acid; more preferably, terephthalic acid.

[0041] According to the present invention, preferably, the diol monomer is ethylene glycol and / or pentanediol; preferably ethylene glycol.

[0042] According to the present invention, preferably, the catalyst is an organic antimony catalyst; preferably ethylene glycol antimony.

[0043] In the present invention, the above-mentioned dibasic acid monomer, diol monomer, spherical nano-silica, polyethylene glycol and catalyst can be obtained commercially, or prepared by the preparation method disclosed in the prior art.

[0044] According to the present invention, the amount of the dibasic acid monomer and the diol monomer can be determined according to the specific requirements of the release film. Preferably, the weight ratio of the dibasic acid monomer to the diol monomer is 1-2.5:1, specifically 1:1, 1.5:1, 2:1, 2.5:1, or any value between these values; more preferably 1.5-1.8:1. The inventors found that under this preferred embodiment, it is beneficial to improve the surface smoothness of the prepared release film.

[0045] According to the present invention, the amount of bis(hydroxyethyl)isophthalate and the catalyst can be determined according to the actual situation. Preferably, in the polyester for the MLCC release film base film, the amount of the catalyst added is 0.01-0.04wt%. The inventors found that the surface of the release film prepared under the above conditions is smoother.

[0046] Preferably, in step S1, the esterification reaction conditions at least include: a temperature of 250-260°C and an absolute pressure of 0.2-0.4MPa. The inventors found that under this preferred embodiment, the spherical silica and polyester can be mixed more evenly during the preparation process, thereby improving the surface smoothness of the release film obtained later. The end condition of the first stage reaction can be determined by the experimenter according to the actual situation, for example, whether to end the first stage reaction is determined according to the amount of water in the reactant I.

[0047] Preferably, in step S2, the polycondensation reaction conditions include: the initial temperature is the esterification reaction temperature, the heating rate is 0.4-0.7°C, and the maximum temperature is 275-285°C. The inventors found that under this preferred embodiment, it is beneficial to improve the surface smoothness of the prepared release film. The conditions for the end of the second stage reaction include: the stirring current reaches a preset value.

[0048] According to the present invention, the preset value of the stirring current can be determined by the test personnel according to the actual situation.

[0049] In the present invention, the method for preparing the release film further comprises: extruding, pelletizing and drying the mixed mixture before stretching into a film, wherein the extrusion, pelletizing and drying methods can be carried out in conventional manners and equipment.

[0050] The third aspect of the present invention provides the use of the MLCC release film described in any technical solution of the first aspect and the MLCC release film prepared by the preparation method described in any technical solution of the second aspect in the preparation of chip-type multilayer ceramic capacitors.

[0051] A fourth aspect of the present invention provides the use of the MLCC release film described in any technical solution of the first aspect and the MLCC release film prepared by the preparation method described in any technical solution of the second aspect in the preparation of smart phones, laptop computers or automobiles.

[0052] According to a particularly preferred embodiment of the present invention, the method for preparing the MLCC release film comprises the following steps:

[0053] S1, reacting terephthalic acid, ethylene glycol and ethylene glycol antimony at a temperature of 250-260° C. and an absolute pressure of 0.2-0.4 MPa; after the reaction, a reactant I is obtained;

[0054] The weight ratio of the terephthalic acid to the ethylene glycol is 1-2.5:1;

[0055] Spherical nano-silicon dioxide having a median particle size d (0.50) of 150-400 nm and a diameter distance of 1.5-2.5 is mixed with an ethylene glycol dispersion solvent to obtain a dispersion of the spherical nano-silicon dioxide;

[0056] S2, mixing the reactant I and the dispersion and reacting them at a heating rate of 0.4-0.7° C.; after the temperature reaches 275-285° C., continuing the reaction at this temperature, and obtaining the polyester for the MLCC release film base film after the stirring current reaches a preset value;

[0057] S3. The MLCC release film base film polyester and conventional polyester are mixed in a mass ratio of 1:0.7-3, extruded, pelletized and dried, and then stretched into a film to obtain the MLCC release film, wherein the content of the spherical nano-silicon dioxide in the release film is 0.1-0.25wt%.

[0058] The above method introduces spherical nano-silica at the end of the esterification reaction under the conditions of a binary reaction system of terephthalic acid and ethylene glycol, and limits the particle size and diameter distance of the spherical nano-silica to achieve uniform dispersion of the spherical nano-silica in the polyester matrix. The MLCC release film base film prepared by melt extrusion and biaxial stretching of the polyester of the present invention has the advantages of uniform dispersion of inorganic powder and small roughness, and the friction coefficient is less than 0.4 to meet the peeling requirements. In addition, the base film matrix component of the release film is still conventional polyester, which is conducive to subsequent recycling.

[0059] The present invention will be described in detail below through examples.

[0060] In the following examples, unless otherwise specified, all other raw materials and reagents used are conventional commercially available products, and their purity is chemically pure.

[0061] The film roughness index is tested by a roughness meter. Ra: arithmetic mean height, which represents the arithmetic mean of the absolute value of the average surface height to the plane; Rz: maximum film height, which represents the distance from the highest point to the lowest point on the surface; Rq: root mean square height of the film, which is equivalent to the parameter of the standard deviation of the distance to the average surface, that is, the standard deviation of the height. The friction coefficient is measured according to GB / T 10006-2021.

[0062] The preparation method of conventional polyester in the following examples and comparative examples is:

[0063] In a 20L general polymerization reactor, 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG) and 1.67g of ethylene glycol antimony catalyst were added, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, the temperature was gradually increased to carry out a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded through a melt pump, pelletized and dried to obtain conventional polyester for base film.

[0064] Example 1

[0065] After spherical nano-silicon dioxide was dispersed in ethylene glycol, a 10 mass % suspension slurry was prepared. The median particle size d(0.5) of the nano-silicon dioxide was 400 nm, and the diameter distance was 1.5. The scanning electron microscope image thereof is shown in FIG. Figure 1 .

[0066] Add 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst to a 20L general polymerization reactor, and carry out a conventional esterification reaction under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction is completed, add 289.15g of suspension slurry. Gradually increase the temperature for a pre-polycondensation reaction for 45min, and carry out a final polycondensation reaction at 280°C. After the stirring current of the reactor reaches the set value, the melt is extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide is 0.50%.

[0067] 2000 g of polyester for MLCC release film base film and 2000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-spherical silica in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0068] Example 2

[0069] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 400 nm and the diameter distance was 1.5.

[0070] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 115.66g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 0.20%.

[0071] 2000 g of polyester for MLCC release film base film and 2000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.10%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0072] Example 3

[0073] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 400 nm and the diameter distance was 1.5.

[0074] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 578.30g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 1.00%.

[0075] 2000 g of polyester for MLCC release film base film and 1400 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.588%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0076] Example 4

[0077] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 400 nm and the diameter distance was 2.5.

[0078] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0079] 2000 g of polyester for MLCC release film base film and 4000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0080] Example 5

[0081] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 150 nm and the diameter distance was 2.0.

[0082] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0083] 2000g of polyester for MLCC release film base film and 6000g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.125%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0084] Example 6

[0085] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 800 nm and the diameter distance was 1.5.

[0086] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 578.3g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0087] 2000 g of polyester for MLCC release film base film and 2000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.50%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0088] Example 7

[0089] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 400 nm and the diameter distance was 1.5.

[0090] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0091] 2000g of polyester for MLCC release film base film and 4000g of conventional polyester were blended and dried as the surface layer of layer A in the ABA three-layer film form, and melt extruded and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the surface layer of the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0092] Example 8

[0093] Spherical nano-silica was dispersed in ethylene glycol to prepare a 10 mass % suspension slurry, the median particle size d(0.5) of the nano-silica was 400 nm, and the diameter distance was 1.5.

[0094] 3000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 0.67g of antimony acetate catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.4MPa and a temperature of 250°C. After the esterification reaction was completed, 289.15g of suspension slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 275°C. After the stirring current of the reactor reached the set value, the melt was extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0095] 2000 g of polyester for MLCC release film base film and 2000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of nano-spherical silica in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0096] Example 9

[0097] Spherical nano-silica was dispersed in ethylene glycol to prepare a 10 mass % suspension slurry, the median particle size d(0.5) of the nano-silica was 400 nm, and the diameter distance was 1.5.

[0098] Add 5000g of terephthalic acid (PTA), 2000g of ethylene glycol (EG), and 2.8g of ethylene glycol antimony catalyst to a 20L general polymerization reactor, and carry out a conventional esterification reaction under the conditions of a gauge pressure of 0.2MPa and a temperature of 260°C. After the esterification reaction is completed, add 289.15g of suspension slurry. Gradually increase the temperature for a pre-polycondensation reaction for 45min, and carry out a final polycondensation reaction at 285°C. After the stirring current of the reactor reaches the set value, the melt is extruded, pelletized, and dried by a melt pump to obtain 5783g of polyester for MLCC release film base film, in which the mass content of nano-silicon dioxide is 0.50%.

[0099] 2000 g of polyester for MLCC release film base film and 2000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of nano-spherical silica in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this embodiment are shown in Table 1, and the measured product parameters are shown in Table 2.

[0100] Example 10

[0101] An MLCC release film was prepared according to the method described in Example 1, except that terephthalic acid was replaced by isophthalic acid.

[0102] Embodiment 11

[0103] An MLCC release film was prepared according to the method described in Example 1, except that ethylene glycol was replaced by pentanediol.

[0104] Comparative Example 1

[0105] Conventional micron-sized silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the silica was 3000 nm and the diameter distance was 1.5.

[0106] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded by a melt pump, pelletized, and dried to obtain 5783g of polyester for base film, in which the mass content of silicon dioxide was 0.50%.

[0107] 2000g of conventional base film polyester and 2000g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of silicon dioxide in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this comparative example are shown in Table 1, and the measured product parameters are shown in Table 2.

[0108] Comparative Example 2

[0109] Spherical nano-silica was dispersed in ethylene glycol to prepare a suspension slurry with a concentration of 10 mass %. The median particle size d (0.5) of the nano-silica was 100 nm, and the diameter distance was 1.5.

[0110] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded by a melt pump, pelletized, and dried to obtain 5783g of polyester for base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0111] 2000g of polyester for base film and 2000g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this comparative example are shown in Table 1, and the measured product parameters are shown in Table 2.

[0112] Comparative Example 3

[0113] After spherical nano-silicon dioxide was dispersed in ethylene glycol, a suspension slurry with a concentration of 10 mass % was prepared. The median particle size d(0.5) of the nano-silicon dioxide was 400 nm, and the diameter distance was 3.0. The scanning electron microscope image thereof is shown in Figure 2 .

[0114] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded by a melt pump, pelletized, and dried to obtain 5783g of polyester for base film, in which the mass content of nano-silicon dioxide was 0.50%.

[0115] 2000g of polyester for base film and 2000g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of spherical nano-silicon dioxide in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this comparative example are shown in Table 1, and the measured product parameters are shown in Table 2.

[0116] Comparative Example 4

[0117] After dispersing the blocky nano-silica in ethylene glycol, a suspension slurry with a concentration of 10 mass % was prepared. The median particle size d(0.5) of the nano-silica was 400 nm, and the diameter distance was 3.0. The scanning electron microscope image thereof is shown in Figure 3 .

[0118] 5000g of terephthalic acid (PTA), 3000g of ethylene glycol (EG), and 1.67g of ethylene glycol antimony catalyst were added to a 20L general polymerization reactor, and a conventional esterification reaction was carried out under the conditions of a gauge pressure of 0.25MPa and a temperature of 255°C. After the esterification reaction was completed, 289.15g of slurry was added. The temperature was gradually increased for a pre-polycondensation reaction for 45min, and a final polycondensation reaction was carried out at 280°C. After the stirring current of the reactor reached the set value, the melt was extruded by a melt pump, pelletized, and dried to obtain 5783g of polyester for base film, in which the mass content of silicon dioxide was 0.50%.

[0119] 2000 g of polyester for base film and 2000 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The mass content of silicon dioxide in the film was 0.25%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this comparative example are shown in Table 1, and the measured product parameters are shown in Table 2.

[0120] Comparative Example 5

[0121] The polyester for MLCC release film base film was prepared in the same manner as in Example 6.

[0122] The MLCC release film base film is directly blended with polyester, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The content of spherical nano-silicon dioxide in the film is 1.00%. The roughness index and friction coefficient of the film are tested. The relevant test parameters in this comparative example are shown in Table 1, and the measured product parameters are shown in Table 2.

[0123] Comparative Example 6

[0124] The polyester for the MLCC release film base film was prepared in the same manner as in Example 1.

[0125] 300 g of polyester for MLCC release film base film and 2700 g of conventional polyester were blended, dried, melt-extruded, and biaxially stretched to obtain an MLCC release film. The content of spherical nano-silicon dioxide in the film was 0.05%. The roughness index and friction coefficient of the film were tested. The relevant test parameters in this comparative example are shown in Table 1, and the measured product parameters are shown in Table 2.

[0126] Table 1

[0127]

[0128]

[0129] Table 2

[0130]

[0131]

[0132] It can be seen from the data in Table 2 that the test results of the film in the embodiment are all within the protection scope of the present invention. Compared with the base film of Comparative Example 1, the roughness index in the embodiment of the present invention is significantly reduced, achieving the effect of preparing the MLCC release base film. It can be seen from the data in Table 2 that the spherical silica used in the present invention has the following characteristics: the shape is spherical, the median particle size d (0.50) is 150nm-800nm, and the diameter distance is 1.2-2.5. The roughness of the film prepared using spherical silica is less than or equal to 25nm, and the minimum can reach 6.5nm; the surface roughness Rq is less than or equal to 50nm, and the minimum can reach 6.9nm; the surface roughness Rz is less than or equal to 293nm, and the minimum can reach 45.3nm; it shows that the prepared film has good flatness, and the friction coefficient is less than 0.4, which ensures that the film can play an anti-adhesion role in the subsequent processing process and is practical. For the shape of spherical silica, although blocky nano-silica can also play a certain role in reducing roughness, the blocky powder will not achieve a monodisperse effect in the actual production process, so the powder size is in a state of varying sizes, and the small-sized particles in the powder will have the adverse effect of increasing crystallization and secondary agglomeration. In addition, large-sized particles will cause the roughness of the film to increase, which is not conducive to the improvement of the flatness of the film. The data in Comparative Example 4 show the side effect of its high roughness. Regarding the particle size range of spherical nano-silica, although small-sized powder is conducive to reducing the roughness of the film, Comparative Example 2 shows that the nano-silica particle size is too small and its internal force is difficult to disperse, which will lead to serious agglomeration, which is manifested as the roughness index of the film becoming larger. In addition, the particle size is too large and its surface roughness is larger. Comparative Example 3 shows that when the particle size distribution of spherical nano-silica is too wide, the large and small particles in the powder will increase the crystallinity and the roughness of the film, so it is not conducive to the preparation of high-quality MLCC release film. Comparative Example 5 shows that when there is too much nano-spherical silica in the film, the roughness will increase and the risk of powder agglomeration inside the film will increase. Comparative Example 6 shows that when there is too little spherical silica, the friction coefficient is too large to be measured, and the subsequent easy peeling effect cannot be achieved. In addition, the large friction coefficient cannot play an anti-adhesion role.

[0133] Taking into account the performance requirements of the MLCC release film, the preparation method of the MLCC release film provided in Examples 1 to 11 is adopted. By adding spherical silica with appropriate particle size and diameter distance during the preparation of the ester for the MLCC release film base film, the surface roughness of the MLCC release film can be effectively reduced, and its viscosity can be reduced so that its friction system meets the requirements, the anti-adhesion effect is achieved, and the subsequent peeling is convenient.

[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A MLCC release film, It is characterized in that The surface roughness Ra of the release film is less than or equal to 25 nm, the surface roughness Rq is less than or equal to 50 nm, the surface roughness Rz is less than or equal to 293 nm, and the friction coefficient is less than or equal to 0.

4.

2. The MLCC release film according to claim 1, It is characterized in that The surface roughness Rp of the release film is less than or equal to 190 nm.

3. The MLCC release film according to claim 1 or 2, It is characterized in that The surface roughness Ra of the release film is less than or equal to 15 nm, the surface roughness Rq is less than or equal to 10 nm, and the surface roughness Rz is less than or equal to 50 nm; Preferably, the surface roughness Ra of the release film is less than or equal to 7 nm, the surface roughness Rq is less than or equal to 7 nm, and the surface roughness Rz is less than or equal to 46 nm.

4. The MLCC release film according to claim 3, It is characterized in that The surface roughness Rp of the release film is less than or equal to 40 nm; Preferably, the surface roughness Rp of the release film is less than or equal to 35 nm.

5. A method for preparing a MLCC release film, It is characterized in that The method comprises the following steps: S1. Under esterification reaction conditions, a dibasic acid monomer, a diol monomer and a catalyst are reacted in a first stage to obtain a reactant I; S2. Under polycondensation reaction conditions, the reactant I and the dispersion containing spherical nano-silicon dioxide are mixed to carry out a second-stage reaction to obtain a polyester for an MLCC release film base film; the median particle size of the spherical nano-silicon dioxide is 150-800 nm, and the diameter distance is 1.2-2.5; S3, mixing the MLCC release film base film polyester and conventional polyester and stretching the mixture into a film to obtain the MLCC release film.

6. The preparation method according to claim 5, It is characterized in that The mass ratio of the polyester for the MLCC release film base film to the conventional polyester is 1:0.7-3.

7. The preparation method according to claim 5 or 6, It is characterized in that In the release film, the addition amount of the spherical nano-silicon dioxide is 0.1-0.6wt%; Preferably, in the release film, the added amount of the spherical nano-silicon dioxide is 0.1-0.25wt%.

8. The preparation method according to claim 5 or 6, It is characterized in that The median particle size of the spherical nano-silicon dioxide is 150-800 nm, and the diameter distance is 1.2-2.5; Preferably, the median particle size of the spherical nano-silicon dioxide is 150-400 nm, and the diameter distance is 1.5-2.

5.

9. Use of the MLCC release film according to any one of claims 1 to 4 or the MLCC release film prepared according to the method according to any one of claims 5 to 8 in the preparation of chip-type multilayer ceramic capacitors.

10. Use of the MLCC release film according to any one of claims 1 to 4 or the MLCC release film prepared according to the method according to any one of claims 5 to 8 in the preparation of smart phones, laptop computers or automobiles.

Citation Information

Patent Citations

  • Low-roughness release film base film and preparation method thereof

    CN113524848A

  • MLCC release film base film and preparation method thereof

    CN114407468A

  • Polyester master batch special for MLCC release film and preparation method of polyester master batch

    CN115322533A

  • Polyester film for capacitor

    JP1998163064A

Cited By

  • Anti-static polyester master batch, preparation method thereof and MLCC release film

    CN121319572A