Multilayer ceramic dielectric capacitor based on continuous electrode and preparation method thereof
Through the sintering process of barium titanate nanoparticles coated with spherical nickel powder and oxide mixed ceramic dielectric material, combined with precisely controlled atmosphere conditions, the problems of nickel electrode oxidation and dielectric layer separation are solved, achieving high capacity and high reliability multi-layer porcelain dielectric capacitor.
Patent Information
- Application Number
- CN202411042805.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
AI Technical Summary
In the sintering process, the electrode layer and the dielectric layer are separated due to the difference in the sintering shrinkage characteristics of the nickel inner electrode and the ceramic dielectric layer, which affects the reliability and capacity of the product. It is difficult for traditional processes to control the oxidation atmosphere. Uniformity, resulting in oxidation cracks and leakage problems.
Barium titanate nanoparticles are used to coat spherical nickel powder and mixed ceramic dielectric materials with glass powder, aluminum trioxide, dysprosium oxide and other oxides. Through high-temperature sintering and atmosphere control, a continuous electrode is formed to prevent nickel electrodes from oxidizing and improve dielectric The insulation performance of the layer, combined with the use of water vapor and hydrogen, accurately regulates the atmosphere in the furnace, ensuring the continuity of the electrode layer and the density of the dielectric layer.
The anti-oxidation of nickel electrodes is achieved, the capacity and product reliability are improved, the oxygen vacancy and leakage problems are reduced, the continuity of the electrode layer and the density of the dielectric layer are enhanced, and the capacity and voltage resistance are improved.
Smart Images

Figure CN118942902A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of capacitors, in particular to a multilayer ceramic capacitor based on continuous electrodes and a preparation method thereof. Background Art
[0002] The continuity of the inner electrode of multilayer ceramic capacitors has an important influence on the electrical properties such as product capacity, loss, insulation resistance, and product reliability. In order to prevent the oxidation of nickel electrodes, multilayer ceramic capacitors with nickel electrodes must be sintered in a reducing atmosphere. However, since the dielectric material is sintered in a completely reducing atmosphere, oxygen vacancies will appear, which will lead to a decrease in insulation performance, and then the reliability of the product will be deteriorated. The ceramic dielectric layer and the nickel inner electrode layer are sintered at the same temperature, but the sintering shrinkage characteristics of the two are very different. When the temperature reaches 900-1000°C, the nickel inner electrode layer shrinks rapidly, while the sintering shrinkage start temperature of the ceramic dielectric layer is about 1100-1200°C. This mismatch in sintering shrinkage will directly lead to obvious separation cracks between the electrode layer and the ceramic dielectric layer. Therefore, in the sintering process, the ceramic dielectric and the nickel inner electrode raw materials must balance the oxidation of the nickel inner electrode and the reduction of the dielectric layer, while ensuring that the nickel electrode is not oxidized, the insulation properties of the dielectric layer and the reliability of the product are also guaranteed.
[0003] The traditional MLCC sintering process usually uses humidification or air ventilation during the reoxidation stage to replenish oxygen to the ceramic body. Because the uniformity and precision of the atmosphere are difficult to control, it is inevitable that the electrode layer will be oxidized to a certain extent. Especially for thin-layer and high-capacity products, this will lead to a series of problems such as a large decrease in capacity and tiny oxidation cracks in the product, affecting the reliability of the product during use. Summary of the invention
[0004] The object of the present invention is to provide a multilayer ceramic capacitor based on continuous electrodes and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a multilayer ceramic capacitor based on continuous electrodes, comprising the following preparation steps:
[0006] (1) barium titanate, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed to obtain a mixed material; the mixed material, polyvinyl alcohol, and a defoamer are mixed in a mass ratio of 1:0.01-0.05:0.0001-0.0004, deionized water is added to a solid content of 20-45%, ball milling is performed for 3-5 hours at a ball-to-material ratio of 5:1, spray granulation is performed, and pressing is performed, the temperature is increased to 600°C at a rate of 5-20°C / min, and the temperature is kept for 1-2 hours, and then the temperature is increased to 1000°C at the same rate, and the temperature is kept for 1-3 hours, and then the temperature is decreased to 600°C at a rate of 8-15°C / min, and then the temperature is naturally cooled to room temperature to obtain a ceramic dielectric material;
[0007] (2) Mixing composite nickel powder, barium titanate oxide mixed powder, water suspension, dispersant, polymer resin, organic solvent, oxidized polyethylene wax, plasticizer, and defoamer, evacuating to a pressure of -0.4 to -0.8 MPa, stirring at 30 to 60 rpm for 30 to 50 min, placing in a high-pressure homogenizer, dispersing at 1000 to 3000 bar for 2 to 5 times, filtering, and taking the filtrate to obtain a nickel inner electrode slurry;
[0008] (3) mixing ethanol, toluene, dispersant, ceramic dielectric material, plasticizer, polymer resin, and defoamer in a mass ratio of 15-35:10-20:0.5-2:100:1-5:4-8:0.001-0.005, stirring at 30-60 rpm for 2-4 hours, grinding at a ball-to-material ratio of 5:1 for 3-5 hours, filtering and collecting the filtrate to obtain a casting slurry;
[0009] (4) Casting the cast slurry into a ceramic diaphragm with a casting thickness of 3 to 12 μm, printing the nickel inner electrode slurry onto the dielectric diaphragm by screen printing to form a dielectric layer, stacking the dielectric layers, stacking 60 layers, isostatically pressing at 100 MPa for 30 min, and then cutting to obtain a green body; degreasing at 250 to 350° C. for 6 to 10 h in a nitrogen atmosphere, heating to 1100 to 1300° C. at a rate of 10 to 50° C. / min in a reducing atmosphere, keeping the temperature for 0.5 to 2 h, the volume ratio of hydrogen to nitrogen in the reducing atmosphere being 0.1 to 2:100, cooling to 1000 to 1100° C., bubbling water vapor, controlling the water volume by MFC, and adding water by high-temperature vaporization of water and mixing with nitrogen carrier gas simultaneously; during the oxidation process, the oxygen analysis potential does not exceed 750 mV, and the oxygen content is 5×10 -9 ~3×10 -6 PPM; oxygen supplement for 1 to 2 hours, chamfer, apply copper terminal electrode slurry on the two opposite end faces of the capacitor, keep warm at 750 to 950°C for 10 to 12 minutes under nitrogen protection, and then undergo surface treatment, metal deposition on nickel barrier layer and tin layer, and finally obtain a multilayer ceramic capacitor with continuous electrodes.
[0010] Furthermore, the particle size of the barium titanate in step (1) is 0.1 to 0.3 μm.
[0011] Furthermore, in step (1), the mass ratio of barium titanate, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate and yttrium oxide is
[0012] 100:0.1~0.5:0.1~1.0:0.1~0.3:0.2~0.9:0.12~0.52:0.1~1.0.
[0013] Furthermore, the preparation method of the composite nickel powder in step (2) is as follows: tetrabutyl titanate, citric acid, and glacial acetic acid are mixed in a volume ratio of 1:2:4, and stirred to obtain a solution A; a barium acetate-glacial acetic acid solution having a concentration of 0.8 to 1.3 mol / L is added in a molar ratio of tetrabutyl titanate to barium acetate of 1:1; after stirring, 1 / 3 to 1 / 2 of the total volume of solution B is added; the solution B contains titanium dioxide with a particle size of 40 to 60 nm, dysprosium oxide with a particle size of 50 to 80 nm, and a mass fraction of 8 The mass ratio of 0-95% ethanol aqueous solution is 1:1:50. Under 400-600W ultrasound, 0.3-0.5 times the mass of the total solution is added with nickel powder with an average particle size of 260-300nm, and the mixture is kept at 40-80℃ for 0.5-3h, then dried at 130-260℃ for 6-10h, then kept at 720-850℃ for 2-5h, and then kept at 550-600℃ for 2-5h under nitrogen atmosphere protection, cooled naturally to room temperature, and ground to an average particle size of 200-300nm.
[0014] Furthermore, in step (2), the mass ratio of the composite nickel powder, barium titanate oxide mixed powder, water suspension, dispersant, polymer resin, organic solvent, oxidized polyethylene wax, plasticizer and defoaming agent is 40-60:3-10:0.005-0.025:0.5-2:2-4:30-45:0.5-2:0.1-1:0.01-0.05.
[0015] Furthermore, the barium titanate oxide mixed powder in step (2) is: barium titanate, zirconium dioxide, bismuth trioxide, zinc oxide, and dysprosium oxide are mixed in a mass ratio of 13-20:0.1-0.8:0.01-4:0.01-0.5:0.01-0.1, and ground to an average particle size of 40-80 nm.
[0016] Furthermore, the aqueous suspension agent in step (2) is a mixture of one or more of Tween 80, maleic acid-acrylic acid sodium salt, calcium lignin sulfonate, isodecanol polyoxyethylene ether, polycarboxylate dispersant SD-819, and sodium lignin sulfonate; and the organic solvent is a mixture of one or more of propylene glycol monomethyl ether, ethylene glycol butyl ether acetate, pineneol, and dihydropineneol.
[0017] Furthermore, the dispersant in steps (2) and (3) is a phosphate dispersant NP-4; the polymer resin is a mixture of one or more of ethyl cellulose, nitrocellulose, polyisocyanate, polyvinyl alcohol, and poly-γ-methylstyrene; and the plasticizer is a mixture of one or more of diethyl phthalate, dibutyl diformate, benzyl benzoate, and citrate.
[0018] Furthermore, the defoaming agent in steps (1), (2) and (3) is a mixture of one or more of dimethylsiloxane, trialkylmelamine, melamine cyanurate chloride, fluorosilicone, ethylene glycol siloxane and octanol.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] Firstly, the present invention wraps a mixed gel of barium titanate oxide on the surface of spherical nickel powder, and after calcination, forms a barium titanate nanoparticle-coated morphology. Due to the presence of a certain supporting structure in the gel, the surface after heat treatment has a certain flatness. At the same time, the nanoparticles on the surface of the nickel powder layer play a barrier role to prevent oxidation of the nickel inner electrode and affect the capacity of the MLCC. Moreover, the spherical nickel powder can be oriented and arranged along the plane direction, and the electrode continuity is good. It can give full play to the ability of barium titanate to inhibit nickel shrinkage, and can also achieve a smaller surface roughness after sintering, so that the number of MLCC stacking is increased to obtain a higher capacitance. Secondly, the present invention mixes oxides such as glass powder, aluminum oxide, and dysprosium oxide with barium titanate to obtain a ceramic dielectric material. During the sintering process, the glass powder gradually melts and fills between the particles to form a liquid bridge, which promotes the particle development. The aluminum oxide can promote the sintering activity of barium titanate ceramics. When barium titanate is sintered in a reducing atmosphere, oxides such as dysprosium oxide and yttrium oxide inhibit grain growth and improve insulation capacity. As the sintering temperature increases, the internal structure changes from porous and loose to dense and uniform, and from a thick loose structure to a dense layered structure. After high-temperature sintering, in the reoxidation stage, humidification and reoxidation are carried out to react with the dielectric layer to reduce oxygen vacancies in the dielectric layer and reduce leakage and breakdown of MLCC under high voltage. Water vapor is introduced in the form of bubbles to control the amount of bubbles added to accurately control the uniformity of the furnace atmosphere. At the same time, trace amounts of hydrogen are introduced to accurately control the furnace atmosphere, so that the product gets enough oxygen while preventing the oxidation of the nickel electrode, thereby ensuring the capacity and reliability of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0022] Figure 1 The invention discloses a multilayer ceramic capacitor with continuous electrodes.
[0023] Figure 2 is a cross-sectional structural diagram of a multilayer ceramic capacitor based on continuous electrodes of the present invention;
[0024] Figure 3 This is a cross-sectional SEM image of the multilayer ceramic capacitor based on continuous electrodes of the present invention and a traditional process MLCC. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] (1) barium titanate with a particle size of 0.3 μm, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed in a mass ratio of 100:0.1:0.2:0.1:0.3:0.12:0.1 to obtain a mixture; the mixture, polyvinyl alcohol, and dimethylsiloxane are mixed in a mass ratio of 1:0.01:0.0001, deionized water is added to a solid content of 20%, ball milled for 3 hours at a ball-to-material ratio of 5:1, spray granulated, pressed into shape, heated to 600°C at 5°C / min, kept warm for 1 hour, then heated to 1000°C at the same speed, kept warm for 2 hours, then cooled to 600°C at 8°C / min, and then naturally cooled to room temperature to obtain a ceramic dielectric material;
[0028] (2) Tetrabutyl titanate, citric acid, and glacial acetic acid are mixed in a volume ratio of 1:2:4, and stirred to obtain solution A. According to the molar ratio of tetrabutyl titanate to barium acetate of 1:1, a barium acetate-glacial acetic acid solution with a concentration of 0.8 mol / L is added, and after stirring, 1 / 3 of the total volume of solution B is added, and the mass ratio of titanium dioxide with a particle size of 40 nm, dysprosium oxide with a particle size of 50 nm, and ethanol aqueous solution with a mass fraction of 80% in solution B is 1:1:50. Under 400W ultrasound, 0.3 times the mass of nickel powder with an average particle size of 300 nm of the total solution is added, and the mixture is kept at 40°C for 0.5 h, and then dried at 130°C for 6 h, and then kept at 720°C for 2 h and then kept at 550°C for 2 h under nitrogen atmosphere protection, and naturally cooled to room temperature, and ground and dispersed to an average particle size of about 300 nm to obtain composite nickel powder;
[0029] (3) barium titanate, zirconium dioxide, bismuth trioxide, zinc oxide, and dysprosium oxide are mixed in a mass ratio of 13:0.2:0.01:0.01:0.025, and ground to an average particle size of 40 nm to obtain a mixed powder of barium titanate oxide; composite nickel powder, mixed powder of barium titanate oxide, sodium maleic acid-acrylate, phosphate dispersant NP-4, ethyl cellulose, propylene glycol monomethyl ether, oxidized polyethylene wax, diethyl phthalate, and dimethylsiloxane are mixed in a mass ratio of 40:3:0.005:0.5:2:30:0.5:0.1:0.01, evacuated to an air pressure of -0.4 MPa, stirred at 30 rpm for 30 min, placed in a high-pressure homogenizer, dispersed twice at 1000 bar, filtered, and the filtrate was taken to obtain a nickel inner electrode slurry;
[0030] (4) Ethanol, toluene, phosphate dispersant NP-4, ceramic dielectric material, diethyl phthalate, ethyl cellulose, and dimethylsiloxane were mixed in a mass ratio of 15:10:0.5:100:1:4:0.001, stirred at 30 rpm for 2 h, ground at a ball-to-material ratio of 5:1 for 3 h, and the filtrate was filtered to obtain a casting slurry;
[0031] (5) The cast slurry is cast into a ceramic diaphragm with a cast thickness of 3 μm. The nickel inner electrode slurry is printed on the dielectric diaphragm by screen printing to form a dielectric layer. The dielectric layers are stacked on each other to form 60 layers. After isostatic pressing at 100 MPa for 30 min, the green body is cut. Degreasing is carried out at 270°C for 6 h in a nitrogen atmosphere. The temperature is increased to 1280°C at a rate of 10°C / min in a reducing atmosphere and kept at this temperature for 0.5 h. The volume ratio of hydrogen to nitrogen in the reducing atmosphere is 0.1:100. The temperature is lowered to 1000°C and water vapor is bubbled in. The amount of water is controlled by MFC. The water is vaporized at high temperature and mixed with nitrogen carrier gas and added simultaneously. During the oxidation process, the oxygen analysis potential does not exceed 750 mV and the oxygen content is 5×10 -9 ~3×10 -6PPM; oxygen supplement for 1 hour, chamfer, apply copper terminal electrode slurry on the two opposite end faces of the capacitor, keep warm at 820℃ for 10 minutes under nitrogen protection, and then go through surface treatment, metal deposition on nickel barrier layer and tin layer, and finally obtain a multilayer ceramic capacitor with continuous electrodes.
[0032] Example 2
[0033] (1) barium titanate with a particle size of 0.3 μm, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed in a mass ratio of 100:0.3:0.15:0.2:0.2:0.32:0.15 to obtain a mixture; the mixture, polyvinyl alcohol, and cyanuric chloride cyanuric acid are mixed in a mass ratio of 1:0.03:0.00025, deionized water is added to a solid content of 32%, ball milling is performed for 4 hours at a ball-to-material ratio of 5:1, spray granulation is performed, and pressing is performed, the temperature is increased to 600° C. at a rate of 10° C. / min, and the temperature is kept for 1.5 hours, and then the temperature is increased to 1000° C. at the same rate, and the temperature is kept for 2 hours, and then the temperature is decreased to 600° C. at a rate of 12° C. / min, and then the temperature is naturally cooled to room temperature to obtain a ceramic dielectric material;
[0034] (2) Tetrabutyl titanate, citric acid, and glacial acetic acid are mixed in a volume ratio of 1:2:4, and stirred to obtain solution A. According to the molar ratio of tetrabutyl titanate to barium acetate of 1:1, a barium acetate-glacial acetic acid solution with a concentration of 1.0 mol / L is added, and after stirring, 1 / 2 of the total volume of solution B is added, and the mass ratio of titanium dioxide with a particle size of 50 nm, dysprosium oxide with a particle size of 70 nm, and ethanol aqueous solution with a mass fraction of 89% in solution B is 1:1:50. Under 500W ultrasound, 0.4 times the mass of nickel powder with an average particle size of 260 nm of the total solution is added, and the mixture is kept at 60°C for 2.5 hours, and then dried at 200°C for 8 hours. Then, under the protection of nitrogen atmosphere, the mixture is kept at 800°C for 3.5 hours, and then kept at 570°C for 3 hours, and naturally cooled to room temperature, and ground and dispersed to an average particle size of about 260 nm to obtain composite nickel powder;
[0035] (3) barium titanate, zirconium dioxide, bismuth trioxide, zinc oxide, and dysprosium oxide are mixed in a mass ratio of 17:0.6:0.03:0.02:0.02, and ground to an average particle size of 60 nm to obtain a mixed powder of barium titanate oxide; composite nickel powder, mixed powder of barium titanate oxide, calcium lignin sulfonate, phosphate dispersant NP-4, polyvinyl alcohol, dihydropinene, oxidized polyethylene wax, citrate, and cyanuric chloride melamine are mixed in a mass ratio of 50:6.5:0.015:1.2:3:37.5:1.1:0.4:0.03, evacuated to an air pressure of -0.6 MPa, stirred at 45 rpm for 40 min, placed in a high-pressure homogenizer, dispersed 3 times at 2000 bar, filtered, and the filtrate was taken to obtain a nickel inner electrode slurry;
[0036] (4) ethanol, toluene, phosphate dispersant NP-4, ceramic dielectric material, citrate, polyvinyl alcohol, and cyanuric chloride melamine were mixed in a mass ratio of 25:15:1.2:100:3:6:0.003, stirred at 45 rpm for 3 h, ground at a ball-to-material ratio of 5:1 for 4 h, and the filtrate was filtered to obtain a casting slurry;
[0037] (5) The cast slurry is cast into a ceramic diaphragm with a casting thickness of 12 μm. The nickel inner electrode slurry is printed on the dielectric diaphragm by screen printing to form a dielectric layer. The dielectric layers are stacked on each other to form 60 layers. After isostatic pressing at 100 MPa for 30 min, the green body is cut. Degreasing is performed at 310°C for 8 h in a nitrogen atmosphere. The temperature is increased to 1280°C at a rate of 20°C / min in a reducing atmosphere and kept at this temperature for 1.2 h. The volume ratio of hydrogen to nitrogen in the reducing atmosphere is 1:100. The temperature is lowered to 1000°C and water vapor is bubbled in. The amount of water is controlled by MFC. The water is vaporized at high temperature and mixed with nitrogen carrier gas and added simultaneously. During the oxidation process, the oxygen analysis potential does not exceed 750 mV and the oxygen content is 5×10 -9 ~3×10 -6 PPM; oxygen supplement for 1.5 hours, chamfer, apply copper terminal electrode slurry on the two opposite end faces of the capacitor, keep warm at 820℃ for 10 minutes under nitrogen protection, and then go through surface treatment, metal deposition on nickel barrier layer and tin layer, and finally obtain a multilayer ceramic capacitor with continuous electrodes.
[0038] Example 3
[0039] (1) barium titanate with a particle size of 0.3 μm, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed in a mass ratio of 100:0.5:0.1:0.3:0.9:0.52:0.1 to obtain a mixture; the mixture, polyvinyl alcohol, and octanol are mixed in a mass ratio of 1:0.05:0.0004, deionized water is added to a solid content of 45%, ball milled for 5 hours at a ball-to-material ratio of 5:1, spray granulated, pressed into shape, heated to 600°C at 20°C / min, kept warm for 2 hours, then heated to 1000°C at the same speed, kept warm for 2 hours, then cooled to 600°C at 15°C / min, and then naturally cooled to room temperature to obtain a ceramic dielectric material;
[0040] (2) Tetrabutyl titanate, citric acid, and glacial acetic acid are mixed in a volume ratio of 1:2:4, and stirred to obtain solution A. According to the molar ratio of tetrabutyl titanate to barium acetate of 1:1, a barium acetate-glacial acetic acid solution with a concentration of 1.3 mol / L is added, and after stirring, 1 / 2 of the total volume of solution B is added, and the mass ratio of titanium dioxide with a particle size of 60 nm, dysprosium oxide with a particle size of 80 nm, and ethanol aqueous solution with a mass fraction of 95% is 1:1:50. Under 600W ultrasound, 0.5 times the mass of nickel powder with an average particle size of 300 nm of the total solution is added, and the mixture is kept at 80°C for 3 hours, and then dried at 260°C for 10 hours. Then, under the protection of nitrogen atmosphere, the mixture is kept at 850°C for 5 hours, and then kept at 600°C for 5 hours, and then naturally cooled to room temperature, and ground and dispersed until the average particle size is about 300 nm to obtain composite nickel powder;
[0041] (3) barium titanate, zirconium dioxide, bismuth trioxide, zinc oxide, and dysprosium oxide are mixed in a mass ratio of 20:0.2:0.04:0.05:0.02, and ground to an average particle size of 80 nm to obtain a mixed powder of barium titanate oxide; composite nickel powder, mixed powder of barium titanate oxide, sodium lignin sulfonate, phosphate dispersant NP-4, poly-γ-methylstyrene, ethylene glycol butyl ether acetate, oxidized polyethylene wax, benzyl benzoate, and octanol are mixed in a mass ratio of 60:10:0.025:2:4:45:2:1:0.05, evacuated to a pressure of -0.8 MPa, stirred at 60 rpm for 50 min, placed in a high-pressure homogenizer, dispersed 5 times at 3000 bar, filtered, and the filtrate was taken to obtain a nickel inner electrode slurry;
[0042] (4) ethanol, toluene, phosphate dispersant NP-4, ceramic dielectric material, benzyl benzoate, poly-γ-methylstyrene, and octanol were mixed in a mass ratio of 35:20:2:100:5:8:0.005, stirred at 60 rpm for 4 h, ground at a ball-to-material ratio of 5:1 for 5 h, and the filtrate was filtered to obtain a casting slurry;
[0043] (5) The cast slurry is cast into a ceramic diaphragm with a casting thickness of 12 μm. The nickel inner electrode slurry is printed on the dielectric diaphragm by screen printing to form a dielectric layer. The dielectric layers are stacked on each other to form 60 layers. After isostatic pressing at 100 MPa for 30 min, the green body is cut. The green body is degreased at 350°C for 10 h in a nitrogen atmosphere. The temperature is increased to 1290°C at a rate of 16°C / min in a reducing atmosphere and kept at this temperature for 2 h. The volume ratio of hydrogen to nitrogen in the reducing atmosphere is 2:100. The temperature is lowered to 1000°C and water vapor is bubbled in. The amount of water is controlled by MFC. The water is vaporized at high temperature and mixed with nitrogen carrier gas and added simultaneously. During the oxidation process, the oxygen analysis potential does not exceed 750 mV and the oxygen content is 5×10 -9 ~3×10 -6PPM; oxygen supplement for 2 hours, chamfer, apply copper terminal electrode slurry on the two opposite end faces of the capacitor, keep warm at 820℃ for 10 minutes under nitrogen protection, and then go through surface treatment, metal deposition on nickel barrier layer and tin layer, and finally obtain a multilayer ceramic capacitor with continuous electrodes.
[0044] Comparative Example 1
[0045] (1) barium titanate with a particle size of 0.3 μm, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed in a mass ratio of 100:0.3:0.15:0.2:0.2:0.32:0.15 to obtain a mixture; the mixture, polyvinyl alcohol, and cyanuric chloride cyanuric acid are mixed in a mass ratio of 1:0.03:0.00025, deionized water is added to a solid content of 32%, ball milling is performed for 4 hours at a ball-to-material ratio of 5:1, spray granulation is performed, and pressing is performed, the temperature is increased to 600° C. at a rate of 10° C. / min, and the temperature is kept for 1.5 hours, and then the temperature is increased to 1000° C. at the same rate, and the temperature is kept for 2 hours, and then the temperature is decreased to 600° C. at a rate of 12° C. / min, and then the temperature is naturally cooled to room temperature to obtain a ceramic dielectric material;
[0046] (2) The composite nickel powder, calcium lignin sulfonate, phosphate dispersant NP-4, polyvinyl alcohol, dihydroterpineol, oxidized polyethylene wax, citrate, and cyanuric chloride melamine were mixed in a mass ratio of 50:0.015:1.2:3:37.5:1.1:0.4:0.03, evacuated to a pressure of -0.6 MPa, stirred at 45 rpm for 40 min, placed in a high-pressure homogenizer, dispersed 3 times at 2000 bar, filtered, and the filtrate was taken to obtain a nickel inner electrode slurry;
[0047] (3) Ethanol, toluene, phosphate dispersant NP-4, ceramic dielectric material, citrate, polyvinyl alcohol, and cyanuric chloride melamine were mixed in a mass ratio of 25:15:1.2:100:3:6:0.003, stirred at 45 rpm for 3 h, ground at a ball-to-material ratio of 5:1 for 4 h, and the filtrate was filtered to obtain a casting slurry;
[0048] (4) Casting the cast slurry into a ceramic diaphragm with a casting thickness of 12 μm, printing the nickel inner electrode slurry onto the dielectric diaphragm by screen printing to form a dielectric layer, superimposing the dielectric layer on the dielectric layer, stacking 60 layers, isostatically pressing at 100 MPa for 30 min, and then cutting to obtain a green body; degreasing at 310°C for 8 h in a nitrogen atmosphere, heating to 1280°C at a rate of 20°C / min in a reducing atmosphere, and keeping warm for 1.2 h, the volume ratio of hydrogen to nitrogen in the reducing atmosphere is 1:100, cooling to 1000°C, supplementing oxygen by controlling the temperature and humidification, controlling the water temperature at 40°C, oxidizing for 5 h, chamfering, coating the copper terminal electrode slurry on the two opposite end faces of the capacitor, keeping warm at 820°C for 10 min under nitrogen protection, and then surface treatment, metal deposition of nickel barrier layer and tin layer, and finally obtaining a multilayer ceramic dielectric capacitor with continuous electrodes.
[0049] Comparative Example 2
[0050] (1) barium titanate with a particle size of 0.3 μm, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed in a mass ratio of 100:0.3:0.15:0.2:0.2:0.32:0.15 to obtain a mixture; the mixture, polyvinyl alcohol, and cyanuric chloride cyanuric acid are mixed in a mass ratio of 1:0.03:0.00025, deionized water is added to a solid content of 32%, ball milling is performed for 4 hours at a ball-to-material ratio of 5:1, spray granulation is performed, and pressing is performed, the temperature is increased to 600° C. at a rate of 10° C. / min, and the temperature is kept for 1.5 hours, and then the temperature is increased to 1000° C. at the same rate, and the temperature is kept for 2 hours, and then the temperature is decreased to 600° C. at a rate of 12° C. / min, and then the temperature is naturally cooled to room temperature to obtain a ceramic dielectric material;
[0051] (2) Tetrabutyl titanate, citric acid, and glacial acetic acid are mixed in a volume ratio of 1:2:4, and stirred to obtain solution A. According to the molar ratio of tetrabutyl titanate to barium acetate of 1:1, a barium acetate-glacial acetic acid solution with a concentration of 1.0 mol / L is added, and after stirring, 1 / 2 of the total volume of solution B is added, and the mass ratio of titanium dioxide with a particle size of 50 nm, dysprosium oxide with a particle size of 70 nm, and ethanol aqueous solution with a mass fraction of 89% in solution B is 1:1:50. Under 500W ultrasound, 0.4 times the mass of nickel powder with an average particle size of 260 nm of the total solution is added, and the mixture is kept at 60°C for 2.5 hours, and then dried at 200°C for 8 hours. Then, under the protection of nitrogen atmosphere, the mixture is kept at 800°C for 3.5 hours, and then kept at 570°C for 3 hours, and naturally cooled to room temperature, and ground and dispersed to an average particle size of 260 nm to obtain composite nickel powder;
[0052] (3) barium titanate, zirconium dioxide, bismuth trioxide, zinc oxide, and dysprosium oxide are mixed in a mass ratio of 17:0.6:0.03:0.02:0.02, and ground to an average particle size of 60 nm to obtain a mixed powder of barium titanate oxide; composite nickel powder, mixed powder of barium titanate oxide, calcium lignin sulfonate, phosphate dispersant NP-4, polyvinyl alcohol, dihydropinene, oxidized polyethylene wax, citrate, and cyanuric chloride melamine are mixed in a mass ratio of 50:6.5:0.015:1.2:3:37.5:1.1:0.4:0.03, evacuated to an air pressure of -0.6 MPa, stirred at 45 rpm for 40 min, placed in a high-pressure homogenizer, dispersed 3 times at 2000 bar, filtered, and the filtrate was taken to obtain a nickel inner electrode slurry;
[0053] (4) ethanol, toluene, phosphate dispersant NP-4, ceramic dielectric material, citrate, polyvinyl alcohol, and cyanuric chloride melamine were mixed in a mass ratio of 25:15:1.2:100:3:6:0.003, stirred at 45 rpm for 3 h, ground at a ball-to-material ratio of 5:1 for 4 h, and the filtrate was filtered to obtain a casting slurry;
[0054] (5) Casting the cast slurry into a ceramic diaphragm with a casting thickness of 12 μm, printing the nickel inner electrode slurry onto the dielectric diaphragm by screen printing to form a dielectric layer, superimposing the dielectric layer on the dielectric layer, stacking 60 layers, isostatically pressing at 100 MPa for 30 min, and then cutting to obtain a green body; degreasing at 310°C for 8 h in a nitrogen atmosphere, heating to 1280°C at a rate of 20°C / min in a reducing atmosphere, and keeping the temperature for 1.2 h. The volume ratio of hydrogen to nitrogen in the reducing atmosphere is 1:100, cooling to 1000°C, supplementing oxygen by adding air, and the ratio of air to nitrogen is 1:20000, chamfering, coating the copper terminal electrode slurry on the two opposite end faces of the capacitor, keeping the temperature at 820°C for 10 min under nitrogen protection, and then surface treatment, metal deposition of nickel barrier layer and tin layer, and finally obtaining a multilayer ceramic dielectric capacitor with continuous electrodes.
[0055] Effect example
[0056] Table 1 below shows the performance analysis results of multilayer ceramic capacitors based on continuous electrodes using Examples 1 to 3 of the present invention and Comparative Examples 1 to 2.
[0057] Table 1
[0058] Dielectric constant Dielectric loss Average capacity (UF) Average withstand voltage(V) Example 1 2861 0.018 1.02 980 Example 2 2897 0.018 1.03 985 Example 3 2795 0.020 1.01 975 Comparative Example 1 2233 0.023 0.82 760 Comparative Example 2 2180 0.023 0.81 790
[0059] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention uses barium titanate composite nanoparticles to coat the surface of the spherical nickel powder, which plays a barrier role, prevents the oxidation of the nickel internal electrode, and affects the capacity of the MLCC, and the spherical nickel powder can be oriented along the plane direction, and the electrode continuity is good. The present invention uses glass powder, aluminum oxide, dysprosium oxide and barium titanate to promote the sintering activity of barium titanate ceramics, and after sintering, water vapor is introduced in the form of bubbles for reoxidation, so that the product obtains sufficient oxygen, while preventing the oxidation of the nickel electrode, ensuring the capacity and reliability of the product.
[0060] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a multilayer ceramic capacitor based on continuous electrodes, characterized in that it comprises the following preparation steps: (1) barium titanate, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate, and yttrium oxide are mixed to obtain a mixed material; the mixed material, polyvinyl alcohol, and a defoaming agent are added in a mass ratio 1:0.01~0.05:0.0001~0.0004, add deionized water to a solid content of 20~45%, ball mill for 3~5 hours at a ball-to-material ratio of 5:1, spray granulate, press mold, heat to 600℃ at 5~20℃ / min, keep warm for 1~2h, then heat to 1000℃ at the same speed, keep warm for 1~3h, then cool to 600℃ at 8~15℃ / min, and naturally cool to room temperature to obtain a ceramic dielectric material; (2) Mixing composite nickel powder, barium titanate oxide mixed powder, water suspension, dispersant, polymer resin, organic solvent, oxidized polyethylene wax, plasticizer, and defoamer, evacuating to a pressure of -0.4 to -0.8 MPa, stirring at 30 to 60 rpm for 30 to 50 min, placing in a high-pressure homogenizer, dispersing at 1000 to 3000 bar for 2 to 5 times, filtering, and taking the filtrate to obtain a nickel inner electrode slurry; (3) mixing ethanol, toluene, dispersant, ceramic dielectric material, plasticizer, polymer resin, and defoamer in a mass ratio of 15-35:10-20:0.5-2:100:1-5:4-8:0.001-0.005, stirring at 30-60 rpm for 2-4 hours, grinding at a ball-to-material ratio of 5:1 for 3-5 hours, filtering and collecting the filtrate to obtain a casting slurry; (4) Casting the cast slurry into a ceramic diaphragm with a casting thickness of 3 to 12 μm, printing the nickel inner electrode slurry onto the dielectric diaphragm by screen printing to form a dielectric layer, stacking the dielectric layers, stacking 60 layers, isostatically pressing at 100 MPa for 30 min, and then cutting to obtain a green body; degreasing at 250 to 350° C. for 6 to 10 h in a nitrogen atmosphere, heating to 1100 to 1300° C. at a rate of 10 to 50° C. / min in a reducing atmosphere, keeping the temperature for 0.5 to 2 h, the volume ratio of hydrogen to nitrogen in the reducing atmosphere being 0.1 to 2:100, cooling to 1000 to 1100° C., bubbling water vapor, controlling the water volume by MFC, and adding water by high-temperature vaporization of water and mixing with nitrogen carrier gas simultaneously; during the oxidation process, the oxygen analysis potential does not exceed 750 mV, and the oxygen content is 5×10 -9 ~3×10 -6 PPM; oxygen supplement for 1 to 2 hours; chamfering, coating copper terminal electrode slurry on the two opposite end faces of the capacitor, keeping warm at 750 to 950°C for 10 to 12 minutes under nitrogen protection, and then surface treatment, metal deposition on nickel barrier layer and tin layer, finally obtaining a multilayer ceramic capacitor with continuous electrodes.
2. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The particle size of the barium titanate in step (1) is 0.1 to 0.3 μm.
3. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The mass ratio of barium titanate, MgO-Al2O3-SiO2 cordierite glass powder, aluminum oxide, dysprosium oxide, silicon dioxide, manganese carbonate and yttrium oxide in step (1) is 100: 0.1-0.5: 0.1-1.0: 0.1-0.3: 0.2-0.9: 0.12-0.52: 0.1-1.
0.
4. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The preparation method of the composite nickel powder in step (2) is as follows: tetrabutyl titanate, citric acid, and glacial acetic acid are mixed in a volume ratio of 1:2:4, and stirred to obtain a solution A; a barium acetate-glacial acetic acid solution having a concentration of 0.8 to 1.3 mol / L is added in a molar ratio of tetrabutyl titanate to barium acetate of 1:1; after stirring, 1 / 3 to 1 / 2 of the total volume of solution B is added; the solution B contains titanium dioxide with a particle size of 40 to 60 nm, dysprosium oxide with a particle size of 50 to 80 nm, and a mass fraction of 80 to 9 The mass ratio of the 5% ethanol aqueous solution is 1:1:
50. Under ultrasound at 400-600W, 0.3-0.5 times the mass of the total solution is added with nickel powder with an average particle size of 260-300nm, and the mixture is kept at 40-80℃ for 0.5-3h, then dried at 130-260℃ for 6-10h, and then kept at 720-850℃ for 2-5h and then kept at 550-600℃ for 2-5h under nitrogen atmosphere protection, cooled naturally to room temperature, and ground to an average particle size of 200-300nm.
5. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The mass ratio of the composite nickel powder, barium titanate oxide mixed powder, water suspension, dispersant, polymer resin, organic solvent, oxidized polyethylene wax, plasticizer and defoamer in step (2) is 40-60:3-10:0.005-0.025:0.5-2:2-4:30-45:0.5-2:0.1-1:0.01-0.
05.
6. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The barium titanate oxide mixed powder in step (2) is: barium titanate, zirconium dioxide, bismuth trioxide, zinc oxide, and dysprosium oxide are mixed in a mass ratio of 13-20:0.1-0.8:0.01-4:0.01-0.5:0.01-0.1, and ground to an average particle size of 40-80 nm.
7. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The aqueous suspension agent in step (2) is a mixture of one or more of Tween 80, maleic acid-acrylic acid sodium salt, calcium lignin sulfonate, isodecanol polyoxyethylene ether, polycarboxylate dispersant SD-819, and sodium lignin sulfonate; the organic solvent is a mixture of one or more of propylene glycol monomethyl ether, ethylene glycol butyl ether acetate, pineneol, and dihydropineneol.
8. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The dispersant in steps (2) and (3) is a phosphate dispersant NP-4; the polymer resin is a mixture of one or more of ethyl cellulose, nitrocellulose, polyisocyanate, polyvinyl alcohol, and poly-γ-methylstyrene; and the plasticizer is a mixture of one or more of diethyl phthalate, dibutyl diformate, benzyl benzoate, and citrate.
9. The method for preparing a multilayer ceramic capacitor based on continuous electrodes according to claim 1, characterized in that: The defoaming agent in steps (1), (2) and (3) is a mixture of one or more of dimethylsiloxane, trialkyl melamine, cyanuric chloride melamine, fluorosilicone, ethylene glycol siloxane and octanol.
Citation Information
Cited By
LTCC (Low Temperature Co-Fired Ceramic) filter for inhibiting sintering shrinkage and preparation method thereof