Control method of hard alloy cobalt magnet

By establishing the relationship between the total carbon and oxygen content of the cemented carbide mixture and the cobalt magnetic value, and adding tungsten powder or carbon black, the problem of performance fluctuations in cemented carbide caused by the difference in raw material batches is solved, and the cobalt magnetic is achieved Accurate control and mechanical performance improvement.

CN118895436APending Publication Date: 2024-11-05CHONGYI ZHANGYUAN TUNGSTEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410922517.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In cemented carbide production, due to the slight differences in chemical composition caused by different raw material batches, the alloy properties such as hardness and wear resistance fluctuate, making it difficult to achieve precise control of cobalt magnetism.

Method used

By establishing the relationship between the total carbon and oxygen content of cemented carbide mixture and the cobalt magnetic value, the ingredients are prepared according to the target cobalt magnetic value and the actual content is detected, and tungsten powder or carbon black is supplemented to control the cobalt magnetic value to achieve the Accurate control.

Benefits of technology

It effectively stabilizes the cobalt magnetic value of cemented carbide, improves the mechanical properties of the alloy, meets practical application needs, and reduces fluctuations in product performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of hard alloy preparation, and particularly relates to a hard alloy cobalt magnetic control method, which comprises the following steps of: establishing a relationship between a cobalt magnetic value of a hard alloy and the total process carbon and oxygen content of a hard alloy mixture based on the total process carbon and oxygen content of the hard alloy mixture and the cobalt magnetic value of the hard alloy in a hard alloy production process; according to the target cobalt magnetic value of the hard alloy to be produced and the corresponding theoretical carbon blending value, blending is carried out to obtain a hard alloy mixture, and the total process carbon content and the total process oxygen content of the hard alloy mixture are obtained through detection, based on the relation between the cobalt magnetic value of the hard alloy and the total process carbon content and the total process oxygen content of the hard alloy mixture, calculating to obtain an actual cobalt magnetic value of the hard alloy obtained by adopting the hard alloy mixture; and based on the relation between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is supplemented, and hard alloy cobalt magnetic control is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cemented carbide preparation, and in particular relates to a control method for cemented carbide cobalt magnets. Background Art

[0002] With the advancement of technology, the control of total carbon in cemented carbide production is becoming more and more stringent. It must be based on the use characteristics of the alloy and the comprehensive performance of the alloy to make the phase region in a specific position (area) in the two-phase region to achieve precise control of the total carbon of the alloy. The introduction of the physical concept of cobalt magnetism has turned the control of carbon in cemented carbide production into the control of cobalt magnetism, that is, the control of the magnetic cobalt content in the alloy; the physical meaning of cobalt magnetism is clear, intuitive, and the inspection is quick and accurate. The control of the product cobalt magnetism can achieve the control of the comprehensive performance of the product. Although the total amount of ingredients in a single batch in cemented carbide production is the same, due to the different batches of raw materials, that is, the chemical composition has slight differences; after the ingredients of different batches of raw materials are calculated, the actual amount of ingredients of each element is different, which leads to fluctuations in the performance of alloy products, among which the most obvious is the fluctuation of product hardness, wear resistance, etc. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a control method for cemented carbide cobalt magnets.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A control method for cemented carbide cobalt magnets, comprising the following steps:

[0006] S1. Based on the total carbon and oxygen content of cemented carbide mixture in the process of cemented carbide production and the cobalt magnetic value of cemented carbide, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of cemented carbide mixture is established;

[0007] S2, preparing a cemented carbide mixture according to the target cobalt magnetic value of the cemented carbide to be produced and its corresponding theoretical carbon content, detecting the total carbon and oxygen content of the cemented carbide mixture during the process of obtaining the cemented carbide mixture, and calculating the actual cobalt magnetic value of the cemented carbide obtained by using the cemented carbide mixture based on the relationship between the cobalt magnetic value of the cemented carbide and the total carbon and oxygen content of the cemented carbide mixture during the process;

[0008] S3. Based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is added to achieve the control of cemented carbide cobalt magnetism.

[0009] As a preferred embodiment of the control method of cemented carbide cobalt magnetism described in the present invention, wherein: in the step S1, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture during the process is: G=M+d×(C+f×O), wherein G is the cobalt magnetic value of cemented carbide, C is the total carbon content of the cemented carbide mixture during the process, and O is the oxygen content of the cemented carbide mixture during the process; M, d, and f are all constants.

[0010] As a preferred embodiment of the method for controlling cemented carbide cobalt magnetism described in the present invention, in step S3, when the actual cobalt magnetism value is greater than the target cobalt magnetism value, tungsten powder is supplemented.

[0011] As a preferred embodiment of the method for controlling cemented carbide cobalt magnetism described in the present invention, in step S3, when the actual cobalt magnetism value is less than the target cobalt magnetism value, carbon black is added.

[0012] As a preferred embodiment of the control method of cemented carbide cobalt magnetism described in the present invention, in step S3, when the actual cobalt magnetism value is greater than the target cobalt magnetism value, the amount of tungsten powder W is added. 钨粉 for:

[0013] W 钨粉 =(C 实际 +f×O 实际 )×H / (C 目标 +f×O 目标 )-H

[0014] Among them, C 实际 is the total carbon content of cemented carbide mixture, O 实际 is the process oxygen content of cemented carbide mixture, H is the mass of cemented carbide mixture, C 目标 is the target process total carbon content of the cemented carbide mix to be produced, O 目标 The target process oxygen content of the cemented carbide mix for the cemented carbide to be produced.

[0015] As a preferred embodiment of the control method of cemented carbide cobalt magnetism of the present invention, in which: in step S3, when the actual cobalt magnetism value is less than the target cobalt magnetism value, the amount of carbon black added W 碳黑 for:

[0016] W 碳黑 =[(C 目标 +f×O 目标 )-(C 实际 +f×O 实际 )]×H / {1-[(C 目标 +f×O 目标 )-f×O 实际 ]}

[0017] Among them, C实际 is the total carbon content of cemented carbide mixture, O 实际 is the process oxygen content of cemented carbide mixture, H is the mass of cemented carbide mixture, C 目标 is the target process total carbon content of the cemented carbide mix to be produced, O 目标 The target process oxygen content of the cemented carbide mix for the cemented carbide to be produced.

[0018] As a preferred solution of the control method of cemented carbide cobalt magnets described in the present invention, the cemented carbide is WC-Co cemented carbide.

[0019] The beneficial effects of the present invention are as follows:

[0020] The present invention provides a control method for cemented carbide cobalt magnetism. Based on the total carbon and oxygen content of a cemented carbide mixture in a cemented carbide production process and the cobalt magnetic value of the cemented carbide, a relationship between the cobalt magnetic value of the cemented carbide and the total carbon and oxygen content of the cemented carbide mixture is established. The cemented carbide mixture is prepared according to a target cobalt magnetic value of the cemented carbide to be produced and its corresponding theoretical carbon content. The total carbon and oxygen content of the cemented carbide mixture is detected. Based on the relationship between the cobalt magnetic value of the cemented carbide and the total carbon and oxygen content of the cemented carbide mixture, an actual cobalt magnetic value of the cemented carbide obtained by using the cemented carbide mixture is calculated. Based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is supplemented to achieve control of the cemented carbide cobalt magnetism, better control the mechanical properties of the cemented carbide, and meet actual application requirements. DETAILED DESCRIPTION

[0021] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] According to one aspect of the present invention, the present invention provides the following technical solution:

[0023] A control method for cemented carbide cobalt magnets, comprising the following steps:

[0024] S1. Based on the total carbon and oxygen content of cemented carbide mixture in the process of cemented carbide production and the cobalt magnetic value of cemented carbide, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of cemented carbide mixture is established;

[0025] S2, preparing a cemented carbide mixture according to the target cobalt magnetic value of the cemented carbide to be produced and its corresponding theoretical carbon content, detecting the total carbon and oxygen content of the cemented carbide mixture during the process of obtaining the cemented carbide mixture, and calculating the actual cobalt magnetic value of the cemented carbide obtained by using the cemented carbide mixture based on the relationship between the cobalt magnetic value of the cemented carbide and the total carbon and oxygen content of the cemented carbide mixture during the process;

[0026] S3. Based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is added to achieve the control of cemented carbide cobalt magnetism.

[0027] Preferably, in step S1, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture during the process is: G=M+d×(C+f×O), wherein G is the cobalt magnetic value of cemented carbide, C is the total carbon content of the cemented carbide mixture during the process, and O is the oxygen content of the cemented carbide mixture during the process; M, d, and f are all constants.

[0028] Preferably, in step S3, when the actual cobalt magnetic value is greater than the target cobalt magnetic value, tungsten powder is supplemented.

[0029] Preferably, in step S3, when the actual cobalt magnetic value is less than the target cobalt magnetic value, carbon black is supplemented.

[0030] Preferably, in step S3, when the actual cobalt magnetic value is greater than the target cobalt magnetic value, the amount of tungsten powder W is added. 钨粉 for:

[0031] W 钨粉 =(C 实际 +f×O 实际 )×H / (C 目标 +f×O 目标 )-H

[0032] Among them, C 实际 is the total carbon content of cemented carbide mixture, O 实际 is the process oxygen content of cemented carbide mixture, H is the mass of cemented carbide mixture, C 目标 is the target process total carbon content of the cemented carbide mix to be produced, O 目标 The target process oxygen content of the cemented carbide mix for the cemented carbide to be produced.

[0033] Preferably, in step S3, when the actual cobalt magnetic value is less than the target cobalt magnetic value, the amount of carbon black added is W 碳黑 for:

[0034] W 碳黑 =[(C 目标 +f×O 目标 )-(C 实际 +f×O 实际)]×H / {1-[(C 目标 +f×O 目标 )-f×O 实际 ]}

[0035] Among them, C 实际 is the total carbon content of cemented carbide mixture, O 实际 is the process oxygen content of cemented carbide mixture, H is the mass of cemented carbide mixture, C 目标 is the target process total carbon content of the cemented carbide mix to be produced, O 目标 The target process oxygen content of the cemented carbide mix for the cemented carbide to be produced.

[0036] Preferably, the cemented carbide is an ultrafine cemented carbide with WC-Co as the main component.

[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0038] Example 1

[0039] A control method for cemented carbide cobalt magnets, comprising the following steps:

[0040] S1. Based on the total carbon and oxygen content of cemented carbide mixture in the process of cemented carbide production and the cobalt magnetic value of cemented carbide, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of cemented carbide mixture is established;

[0041] The total carbon value and oxygen content average of three batches of process products (WC-6Co ultrafine tungsten carbide cemented carbide) were obtained, and the cobalt magnetic value of the corresponding products was obtained:

[0042] C1=5.7975wt%, O1=0.5625wt%, G1=4.46%

[0043] C2=5.7975wt%, O2=0.525wt%, G2=4.54%

[0044] C3=5.815wt%, O3=0.455wt%, G3=4.97%

[0045] The relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture is:

[0046] 4.46%=M+d×(5.7975%+0.5625%×f)……①

[0047] 4.54%=M+d×(5.7975%+0.525%×f)……②

[0048] 4.97%=M+d×(5.815%+0.455%×f)……③

[0049] From ①②③, we can solve M, d, and f as follows:

[0050] M = -87.27%;

[0051] d = 16.03;

[0052] f = -0.133;

[0053] S2. According to the target cobalt magnetic value of the hard alloy to be produced of 4.97% and its corresponding theoretical carbon content of 5.82wt%, 240kg of hard alloy mixture is prepared. The total carbon and oxygen contents of the hard alloy mixture are detected as follows: C 实际 5.815wt%, O 实际 0.5525wt%, based on the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture, the actual cobalt magnetic value G of the cemented carbide obtained by using the cemented carbide mixture is calculated. 实际 = -87.27% + 16.03 × (5.815% - 0.5525% × 0.133) = 4.767%;

[0054] S3. Based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is added to achieve the control of cemented carbide cobalt magnetism.

[0055] Because the actual cobalt magnetic value is less than the target cobalt magnetic value;

[0056] Therefore, the amount of carbon black added W 碳黑 for:

[0057] W 碳黑 =[(C 目标 +f×O 目标 )-(C 实际 +f×O 实际 )]×H / {1-[(C 目标 +f×O 目标 )-f×O 实际 ]}

[0058] =[(5.815%-0.133×0.455%)-(5.815%-0.5525%×0.133)]

[0059] ×240kg / {1-[(5.815%-0.133×0.455%)+0.133×0.5525%]}=0.032kg.

[0060] The cobalt magnetic value of the product obtained after adding carbon black is 4.98%, which is basically consistent with the target cobalt magnetic value.

[0061] Example 2

[0062] A control method for cemented carbide cobalt magnets, comprising the following steps:

[0063] S1. Based on the total carbon and oxygen content of cemented carbide mixture in the process of cemented carbide production and the cobalt magnetic value of cemented carbide, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of cemented carbide mixture is established;

[0064] The total carbon value and oxygen content average of three batches of process products (WC-6Co ultrafine tungsten carbide cemented carbide) were obtained, and the cobalt magnetic value of the corresponding products was obtained:

[0065] C1=5.7975wt%, O1=0.5625wt%, G1=4.46%

[0066] C2=5.7975wt%, O2=0.525wt%, G2=4.54%

[0067] C3=5.815wt%, O3=0.455wt%, G3=4.97%

[0068] The relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture is:

[0069] 4.46%=M+d×(5.7975%+0.5625%×f)……①

[0070] 4.54%=M+d×(5.7975%+0.525%×f)……②

[0071] 4.97%=M+d×(5.815%+0.455%×f)……③

[0072] From ①②③, we can solve M, d, and f as follows:

[0073] M = -87.27%;

[0074] d = 16.03;

[0075] f = -0.133;

[0076] S2. According to the target cobalt magnetic value of the hard alloy to be produced of 4.97% and its corresponding theoretical carbon content of 5.82wt%, 240kg of hard alloy mixture is prepared. The total carbon and oxygen contents of the hard alloy mixture are detected as follows: C 实际 5.82wt%, O 实际0.43wt%, based on the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture, the actual cobalt magnetic value G of the cemented carbide obtained by using the cemented carbide mixture is calculated. 实际 = -87.27% + 16.03 × (5.82% - 0.43% × 0.133) = 5.107%;

[0077] S3. Based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is added to achieve the control of cemented carbide cobalt magnetism.

[0078] Because the actual cobalt magnetic value is greater than the target cobalt magnetic value;

[0079] The amount of tungsten powder to be added 钨粉 for:

[0080] W 钨粉 =(C 实际 +f×O 实际 )×H / (C 目标 +f×O 目标 )-H

[0081] =(5.82wt%-0.43%×0.133)×240 / (5.815%-0.133×0.455%)-240kg=0.351kg.

[0082] The cobalt magnetic value of the product obtained after supplementing with tungsten powder is 4.96%, which is basically consistent with the target cobalt magnetic value.

[0083] The present invention establishes the relationship between the cobalt magnetic value of cemented carbide and the process total carbon and oxygen content of the cemented carbide mixture based on the process total carbon and oxygen content of the cemented carbide mixture in the cemented carbide production process and the cobalt magnetic value of the cemented carbide, mixes the cemented carbide mixture according to the target cobalt magnetic value of the cemented carbide to be produced and its corresponding theoretical carbon content, detects the process total carbon and oxygen content of the cemented carbide mixture, and calculates the actual cobalt magnetic value of the cemented carbide obtained by using the cemented carbide mixture based on the relationship between the cobalt magnetic value of the cemented carbide and the process total carbon and oxygen content of the cemented carbide mixture; based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is supplemented to achieve control of the cobalt magnetism of the cemented carbide, better control the mechanical properties of the cemented carbide, and meet the actual application needs.

[0084] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A control method for cemented carbide cobalt magnets, characterized in that: The steps include: S1. Based on the total carbon and oxygen content of cemented carbide mixture in the process of cemented carbide production and the cobalt magnetic value of cemented carbide, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of cemented carbide mixture is established; S2, preparing a cemented carbide mixture according to the target cobalt magnetic value of the cemented carbide to be produced and its corresponding theoretical carbon content, detecting the total carbon and oxygen content of the cemented carbide mixture during the process of obtaining the cemented carbide mixture, and calculating the actual cobalt magnetic value of the cemented carbide obtained by using the cemented carbide mixture based on the relationship between the cobalt magnetic value of the cemented carbide and the total carbon and oxygen content of the cemented carbide mixture during the process; S3. Based on the relationship between the actual cobalt magnetic value and the target cobalt magnetic value, tungsten powder or carbon black is added to achieve the control of cemented carbide cobalt magnetism.

2. The control method of cemented carbide cobalt magnet according to claim 1, characterized in that: In the step S1, the relationship between the cobalt magnetic value of cemented carbide and the total carbon and oxygen content of the cemented carbide mixture during the process is: G=M+d×(C+f×O), wherein G is the cobalt magnetic value of cemented carbide, C is the total carbon content of the cemented carbide mixture during the process, and O is the oxygen content of the cemented carbide mixture during the process; M, d, and f are all constants.

3. The control method of cemented carbide cobalt magnet according to claim 1, characterized in that: In the step S3, when the actual cobalt magnetic value is greater than the target cobalt magnetic value, tungsten powder is supplemented.

4. The control method of cemented carbide cobalt magnet according to claim 1, characterized in that: In step S3, when the actual cobalt magnetic value is less than the target cobalt magnetic value, carbon black is added.

5. The control method of cemented carbide cobalt magnet according to claim 1, characterized in that: In step S3, when the actual cobalt magnetic value is greater than the target cobalt magnetic value, the amount of tungsten powder W is added. 钨粉 for: W 钨粉 =(C 实际 +f×O 实际 )×H / (C 目标 +f×O 目标 )-H Among them, C 实际 is the total carbon content of cemented carbide mixture, O 实际 is the process oxygen content of cemented carbide mixture, H is the mass of cemented carbide mixture, C 目标 is the target process total carbon content of the cemented carbide mix to be produced, O 目标 The target process oxygen content of the cemented carbide mix for the cemented carbide to be produced.

6. The control method of cemented carbide cobalt magnet according to claim 1, characterized in that: In step S3, when the actual cobalt magnetic value is less than the target cobalt magnetic value, the amount of carbon black added is W 碳黑 for: W 碳黑 =[(C 目标 +f×O 目标 )-(C 实际 +f×O 实际 )]×H / {1-[(C 目标 +f×O 目标 )-f×O 实际 ]} Among them, C 实际 is the total carbon content of cemented carbide mixture, O 实际 is the process oxygen content of cemented carbide mixture, H is the mass of cemented carbide mixture, C 目标 is the target process total carbon content of the cemented carbide mix to be produced, O 目标 The target process oxygen content of the cemented carbide mix for the cemented carbide to be produced.

7. The control method of cemented carbide cobalt magnet according to claim 1, characterized in that: The cemented carbide is WC-Co cemented carbide.