Production method of vanadium-chromium-tin-aluminum intermediate alloy

By mixing V2O5, SnO2, Cr2O3, aluminum powder and slag-making agent and processing it in a smelting furnace, the impurity control problem in vanadium chromium tin aluminum intermediate alloy is solved, efficient and low-cost production is achieved, and the performance of titanium alloy is met. Stable demand.

CN118895438APending Publication Date: 2024-11-05PANGANG GROUP VANADIUM & TITANIUM RESOURCES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411103567.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing vanadium chromium tin aluminum intermediate alloy production process is difficult to control the impurity element content, resulting in unstable performance of titanium alloys and high production costs, making it difficult to meet international advanced technical standards.

Method used

V2O5, SnO2, Cr2O3, aluminum powder and slag-making agent are mixed to obtain furnace material, added to the smelting furnace to lay and ignite the ignition agent, and after cooling, the slag and surface impurities are cleaned, crushed and sieved to obtain uniform and high-purity vanadium chromium Tin aluminum intermediate alloy.

Benefits of technology

The performance stability and purity of vanadium chromium tin aluminum intermediate alloy are improved, production costs are reduced, production efficiency is improved, and the production of vanadium chromium tin aluminum intermediate alloy is more efficient and economical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895438A_ABST
    Figure CN118895438A_ABST
Patent Text Reader

Abstract

The invention relates to the field of special alloy production, and provides a production method of a vanadium-chromium-tin-aluminum intermediate alloy, which comprises the following steps: uniformly mixing V2O5, SnO2, Cr2O3, aluminum powder and a slag former to obtain a furnace charge; the furnace burden is added into a smelting furnace, an ignition agent is laid and ignited, and separated furnace slag and alloy liquid are obtained; slag is cleaned after cooling, solidified alloy liquid is taken out, impurities on the surface of the alloy liquid are cleaned, sand blasting is conducted, and alloy blocks are obtained; and the alloy blocks are crushed and screened, and the vanadium-chromium-tin-aluminum intermediate alloy is obtained. According to the method, the vanadium-chromium-tin-aluminum intermediate alloy is more uniform, the performance stability of the vanadium-chromium-tin-aluminum intermediate alloy is improved, impurities in the vanadium-chromium-tin-aluminum intermediate alloy are effectively removed, the impurity content of the vanadium-chromium-tin-aluminum intermediate alloy is reduced, the purity of the vanadium-chromium-tin-aluminum intermediate alloy is improved, the production efficiency is improved, and the production cost is reduced; and the production of the vanadium-chromium-tin-aluminum intermediate alloy is more efficient and economical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of special alloy production, and more specifically to a production method of a vanadium-chromium-tin-aluminum master alloy. Background Art

[0002] With the rapid development of high-end equipment such as aerospace, frame beams and other load-bearing structural parts for aviation and military industries have put forward higher requirements for the specific strength, specific stiffness and other comprehensive properties of titanium alloys. High-strength and toughness titanium alloys are used as structural parts in parts that require high strength and toughness such as aviation, aerospace and military industries, which can further improve the specific strength and specific stiffness of titanium alloys to achieve greater weight reduction. Among them, V-Cr-Sn-Al is an important intermediate alloy raw material for smelting high-strength and high-toughness β titanium alloys. Through the optimization of the introduction form (intermediate alloy), smelting, forging and heat treatment processes of various alloy elements, this type of alloy is expected to become a key structural material in the field of aerospace JG. TB19 alloy is a new type of high-strength, high-toughness, corrosion-resistant near-β titanium alloy developed by Northwest Institute of Nonferrous Metals in 2000. Its nominal composition is Ti-3Al-5Mo-5V-4Cr-2Zr. The alloy has a good match between high strength, high fracture toughness and good plasticity, and at the same time has comprehensive properties such as weldability and resistance to seawater corrosion, erosion corrosion and stress corrosion. The alloy has good processing performance, high strength, high toughness and excellent seawater corrosion resistance. It has broad application prospects in aviation, aerospace, navigation and other fields, and is particularly suitable for making ship materials.

[0003] Although my country has made great progress in the research of high-strength and high-toughness titanium alloys, there is still a large gap in the titanium alloy materials used in high-end aerospace parts in my country compared with the United States, Russia and other aerospace titanium alloy production powerhouses. The main bottlenecks in development are: (1) The domestic foundation is poor and the innovation and development capabilities are insufficient. High-end titanium alloy products are subject to the titanium alloy powerhouses such as the United States and Russia; (2) The introduction of multiple alloying elements has resulted in the composition, structure and performance of titanium alloys being unable to stably and reliably meet the requirements of international advanced technical standards; (3) From product research and development (localization), industrial production, engineering application to feedback optimization, a virtuous circle has not been formed, and there is no way to improve and enhance.

[0004] The smelting of TB5 titanium alloy requires the addition of vanadium-chromium-tin-aluminum master alloy to introduce the elements of aluminum, vanadium, tin, and chromium, but the production process of vanadium-chromium-tin-aluminum master alloy mainly includes oxidation-reduction method and metal material method. The oxidation-reduction method has a lower production cost but it is more difficult to control the inclusions in the alloy, while the metal material method has a high alloy purity but a higher production cost. The content of C, H, O, and N elements in the vanadium-chromium-tin-aluminum master alloy has an important influence on the performance of the titanium alloy. If the content of these elements is not strictly controlled, it is very easy to have an adverse effect on the performance of the titanium alloy. The traditional vanadium-aluminum alloy production process is insufficient in controlling the content of these impurity elements. At the same time, the shapes and physical and chemical properties of the alloys produced are different, and the uniformity of the smelting composition is not easy to control, which makes it difficult to apply in the smelting market of TB5 titanium alloy. Summary of the invention

[0005] In view of this, the present invention proposes a method for producing a vanadium-chromium-tin-aluminum master alloy, which can provide multiple alloying elements such as vanadium, chromium, tin, and aluminum for titanium alloy smelting at one time, and the smelting composition is easy to control and the alloy yield is high.

[0006] Based on the above purpose, the present invention provides a method for producing a vanadium-chromium-tin-aluminum master alloy, comprising the following steps: S1. Mix V2O5, SnO2, Cr2O3, aluminum powder and slag-forming agent to obtain a charge; S2. The charge is added to the smelting furnace, the ignition agent is laid and ignited to obtain separated slag and alloy liquid; S3. After cooling, clean the slag, remove the solidified alloy liquid, clean the impurities on the surface of the alloy liquid and sandblast to obtain an alloy block; S4. Crushing and screening the alloy block to obtain a vanadium-chromium-tin-aluminum intermediate alloy.

[0007] In some embodiments, in step S1, the V2O5 grade is ≥99.0%, the SnO2 grade is ≥99.0%, the Cr2O3 grade is ≥99.0%, and the aluminum powder purity is ≥99.7%.

[0008] In some embodiments, in step S1, the block size of V2O5 is ≤3mm, the particle size of SnO2 is ≤1mm, the particle size of Cr2O3 is ≤1mm, and the particle size of aluminum powder is ≤2mm.

[0009] In some embodiments, in step S2, the alloy liquid is deposited at the bottom of the smelting furnace, and the slag floats on the alloy liquid.

[0010] In some embodiments, in step S3, the cooling requires the smelting furnace to cool for 48 hours, and the temperature inside the furnace is <50°C.

[0011] In some embodiments, in step S4, the step of crushing and screening the alloy block to obtain the vanadium-chromium-tin-aluminum master alloy comprises: Crushing and screening the alloy block to obtain alloy particles of required particle size; Through manual or machine sorting, alloy particles with oxide film are removed; The qualified alloy particles are packed in barrels and sealed to obtain vanadium-chromium-tin-aluminum master alloy.

[0012] In some embodiments, in step S2, the step of adding the charge into the smelting furnace and laying and igniting the ignition agent comprises: Add the prepared charge into the smelting furnace and arrange it evenly; Spread the ignition material evenly on the surface of the charge; The ignition charge is ignited.

[0013] In some embodiments, in step S3, the step of cleaning impurities on the surface of the alloy liquid and sandblasting includes: Clean impurities on the surface of alloy liquid; Remove the defective parts of surface slag inclusions; Clean the oxidized surface by sandblasting; After sandblasting, the surface is inspected to ensure that the desired surface roughness requirements are met.

[0014] In some embodiments, the smelting furnace uses a split graphite crucible.

[0015] In some embodiments, the smelting furnace is composed of a furnace bottom and a plurality of combinable furnace bodies, and the plurality of combinable furnace bodies and / or the furnace bottom are connected by bolts or snaps.

[0016] The present invention has at least the following beneficial technical effects: The invention provides a production method of a vanadium-chromium-tin-aluminum master alloy, which comprises: mixing V2O5, SnO2, Cr2O3, aluminum powder and a slag-forming agent to obtain a furnace charge; adding the furnace charge into a smelting furnace, laying and igniting an ignition agent to obtain separated slag and alloy liquid; cleaning the slag after cooling, taking out the solidified alloy liquid, cleaning impurities on the surface of the alloy liquid and sandblasting to obtain an alloy block; crushing and screening the alloy block to obtain a vanadium-chromium-tin-aluminum master alloy.

[0017] The present invention makes the vanadium-chromium-tin-aluminum master alloy more uniform, improves the performance stability of the vanadium-chromium-tin-aluminum master alloy, effectively removes impurities in the vanadium-chromium-tin-aluminum master alloy, reduces the impurity content of the vanadium-chromium-tin-aluminum master alloy, improves the purity of the vanadium-chromium-tin-aluminum master alloy, improves production efficiency, reduces production costs, and makes the production of the vanadium-chromium-tin-aluminum master alloy more efficient and economical. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 A flow chart showing a method for producing a vanadium-chromium-tin-aluminum master alloy according to an embodiment of the present invention is shown.

[0019] Figure 2 A flow chart of an embodiment of a method for producing a vanadium-chromium-tin-aluminum master alloy according to an embodiment of the present invention is shown.

[0020] Figure 3 A structural diagram of a smelting furnace for a method for producing a vanadium-chromium-tin-aluminum master alloy according to an embodiment of the present invention is shown.

[0021] Among them, 1. Combinable furnace body; 2. Furnace bottom. DETAILED DESCRIPTION

[0022] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0023] In addition, reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0024] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as in the context of the prior art, and will not be interpreted with an idealized or overly formal meaning unless specifically defined as in the embodiments of this application.

[0025] The present invention proposes a method for producing a vanadium-chromium-tin-aluminum master alloy. Figure 1 and Figure 2 , including the following steps: S1. Mix V2O5, SnO2, Cr2O3, aluminum powder and slag-forming agent to obtain a charge; S2. The charge is added to the smelting furnace, the ignition agent is laid and ignited to obtain separated slag and liquid alloy; S3. After cooling, the slag is cleaned, the solidified alloy liquid is removed, impurities on the surface of the alloy liquid are cleaned and sandblasted to obtain an alloy block; S4. Crushing and screening the alloy block to obtain a vanadium-chromium-tin-aluminum master alloy.

[0026] The present invention can provide vanadium, chromium, tin, aluminum and other alloying elements for titanium alloy smelting at one time, so that the vanadium-chromium-tin-aluminum master alloy is more uniform, the performance stability of the vanadium-chromium-tin-aluminum master alloy is improved, impurities in the vanadium-chromium-tin-aluminum master alloy are effectively removed, and the impurity content of the vanadium-chromium-tin-aluminum master alloy is reduced. The smelting composition is easy to control, the alloy yield is high, the purity of the vanadium-chromium-tin-aluminum master alloy is improved, the production efficiency is improved, the production cost is reduced, and the production of the vanadium-chromium-tin-aluminum master alloy is more efficient and economical.

[0027] In some embodiments, the V2O5 grade is ≥99.0%, the SnO2 grade is ≥99.0%, the Cr2O3 grade is ≥99.0%, and the aluminum powder purity is ≥99.7%.

[0028] The grade restriction of raw materials can ensure that the raw materials entering the production process have a relatively high purity or content, requiring fewer refining and purification steps during the processing, thereby improving production efficiency. The grade of raw materials directly affects the performance and quality of the final product. Selecting the right raw material grade can ensure that the final product has stable quality and performance to meet customer needs and industry standards. The use of high-grade raw materials can reduce energy consumption and the use of chemical reagents during refining and purification, thereby reducing production costs. In addition, high-grade raw materials can also reduce the generation of waste in the production process, further reducing the cost of waste treatment.

[0029] In some embodiments, the block size of the V2O5 is ≤3mm, the particle size of the SnO2 is ≤1mm, the particle size of the Cr2O3 is ≤1mm, and the particle size of the aluminum powder is ≤2mm.

[0030] Raw materials with smaller particle sizes enable accurate batching and uniform mixing of the charge, which can react smoothly and quickly, and the reaction is fully completed, thereby obtaining an alloy with stable composition. Particle size restriction can ensure that the raw material particles are uniform in size, which is conducive to more uniform distribution and reaction in chemical reactions or metallurgical processes. Smaller particles have a large surface area, which increases the contact area with other raw materials or reactants, thereby improving the reaction rate and efficiency. Raw materials with uniform particle size help to obtain more consistent product performance and quality during processing. It avoids problems such as local overheating and uneven reaction caused by large differences in raw material particle size, and improves the uniformity and stability of the product. Particle size restriction helps to avoid problems such as blockage and accumulation caused by excessively large raw material particles during processing, and reduces the probability of production accidents. Raw materials with uniform particle size are easier to operate and control in subsequent processing (such as screening, mixing, pressing, etc.).

[0031] In some embodiments, see Figure 3 The smelting furnace uses a split graphite crucible.

[0032] Split graphite crucibles are usually designed and manufactured with safety and stability in mind. They have a small bottom and need to be heated on a graphite pad or mud triangle, which helps avoid thermal stress concentration and damage caused by direct heating. At the same time, their high corrosion resistance can also reduce safety issues caused by chemical reactions. The high thermal conductivity and low thermal expansion coefficient of the graphite crucible enable it to use energy more efficiently and reduce energy waste during use.

[0033] In some embodiments, see Figure 3 The smelting furnace includes a furnace bottom 2 and a plurality of combinable furnace bodies 1. The plurality of combinable furnace bodies 1 and / or the furnace bottom 2 can be connected using bolts or snaps.

[0034] The design of the split graphite crucible allows it to be disassembled and replaced individually, which greatly simplifies the maintenance and replacement process. When part of the crucible is damaged or needs to be replaced, there is no need to replace the entire crucible, only the damaged part needs to be replaced, reducing maintenance costs and time. The split graphite crucible can be combined and matched according to different process requirements to meet different smelting and melting needs. This flexibility makes the split graphite crucible widely used in a variety of industrial fields. The graphite crucible itself has excellent properties such as high temperature resistance, good thermal conductivity, and strong corrosion resistance, and the split design further improves its service life. Since the damaged part can be replaced separately, the service life of the entire crucible can be effectively extended.

[0035] In some embodiments, the alloy liquid is deposited at the bottom of the smelting furnace, and the slag floats on the alloy liquid.

[0036] After the ignition charge is ignited, the charge reacts rapidly and violently. All the charge generally reacts within 2 minutes. The slag and alloy liquid produced by smelting are separated in the furnace defined by the multiple combinable furnace bodies 1. The alloy liquid settles at the bottom of the furnace bottom 2, and the slag floats on the alloy. The surface of the alloy liquid is wrapped and protected by the slag produced by smelting to prevent oxidation pollution of the alloy by the outside air.

[0037] The effective separation of slag and alloy liquid can prevent impurities in the slag from entering the alloy liquid, thereby reducing the pollution of the alloy liquid and improving its purity. This will help improve the performance and quality of the product, including strength, ductility and corrosion resistance, and at the same time prevent the slag from adhering to the inside of the smelting equipment, reducing equipment wear and corrosion, thereby extending the service life of the equipment. Ensure the smooth progress of the smelting process, reduce downtime caused by equipment failure or slag cleaning, and improve production efficiency.

[0038] In some embodiments, the cooling requires the smelting furnace to cool for 48 hours with the temperature inside the furnace <50°C.

[0039] When VCrSnAl master alloy is in contact with oxygen in the air at high temperature, it is easy to undergo oxidation reaction, resulting in the formation of an oxide layer on the surface of VCrSnAl master alloy, which not only affects the appearance of VCrSnAl master alloy, but also may affect its performance and quality. By letting the furnace cool for a period of time, the temperature of VCrSnAl master alloy can be reduced, and its reaction rate with oxygen can be reduced, thereby preventing the oxidation of VCrSnAl master alloy. Thermal stress will be generated during the rapid cooling process, resulting in cracks or deformation inside the VCrSnAl master alloy. Cooling the furnace for a period of time can slowly cool down the VCrSnAl master alloy, reduce the generation of thermal stress, and thus maintain the integrity and stability of the VCrSnAl master alloy.

[0040] In some embodiments, the step of crushing and screening the alloy block to obtain the vanadium-chromium-tin-aluminum master alloy comprises: Crushing and screening the alloy block to obtain alloy particles of required particle size; Through manual or machine sorting, alloy particles with oxide film are removed; The qualified alloy particles are packed in barrels and sealed to obtain vanadium-chromium-tin-aluminum master alloy.

[0041] After the alloy block is crushed and screened, particles or block materials of uniform size and meeting the requirements can be obtained. These materials can be more evenly distributed and reacted in subsequent smelting, smelting, casting and other processes, thereby improving the efficiency of the entire production process. Crushing and screening can remove impurities and unqualified materials in the vanadium chromium tin aluminum master alloy block, making the final product purer. In addition, by controlling the size and distribution of the vanadium chromium tin aluminum master alloy particles, the physical and chemical properties of the vanadium chromium tin aluminum master alloy, such as hardness, strength, toughness, etc., can also be improved, thereby improving the quality of the product. The vanadium chromium tin aluminum master alloy particles after crushing and screening have a smaller volume and a larger specific surface area, which are easier to store and transport. This not only saves storage space, but also reduces transportation costs and time.

[0042] In some embodiments, the step of adding the charge into the smelting furnace and laying and igniting the ignition agent comprises: Add the prepared charge into the smelting furnace and arrange it evenly; Spread the ignition material evenly on the surface of the charge; The ignition charge is ignited.

[0043] When the ignition agent is evenly laid, the heat can be more evenly distributed throughout the ignition area, ensuring consistency and stability in the ignition process. This helps to quickly and effectively start the combustion process and improve ignition efficiency. This facilitates rapid reaction of the charge. Unevenly laid ignition agent may cause local overheating or uneven combustion, increasing the risk of fire or explosion. Evenly laid ignition agent can ensure uniform distribution of heat and combustion process, reducing these safety risks. Uneven ignition may cause local overheating of equipment, accelerating wear and aging of equipment. Evenly laid ignition agent can ensure that the equipment operates at a stable and uniform temperature, extending the service life of the equipment.

[0044] In some embodiments, the step of cleaning impurities on the surface of the alloy liquid and sandblasting includes: Clean impurities on the surface of alloy liquid; Remove the defective parts of surface slag inclusions; Clean the oxidized surface by sandblasting; After sandblasting, the surface is inspected to ensure that the desired surface roughness requirements are met.

[0045] There are some defects on the surface of the alloy block, such as scratches, grooves, protrusions, etc. Sandblasting can effectively remove these defects, restore the surface to a smooth and appropriate roughness, and expose a new metal surface, which helps to improve the production efficiency of the alloy block. The present invention is further described below by means of specific examples.

[0046] Example 1: Please refer to Figure 1 , Figure 2 and Figure 3 , select 5kg of 99.5% powdered vanadium pentoxide (particle size ≤ 1mm), 0.783kg of 99.5% purity SnO2, 1.05kg of 99.0% purity Cr2O3, 3.38kg of 99.5% purity aluminum particles (particle size ≤ 2mm), and 1.2kg of lime for slag making. After accurately adding, mix them thoroughly and evenly in a mixer.

[0047] according to Figure 3 It is required to prepare the smelting furnace and keep it dry.

[0048] The prepared charge was placed in the smelting furnace, the ignition agent was arranged, and the smelting was ignited. The reaction time was about 30 seconds. After standing and cooling naturally for 24 hours, the furnace was dismantled, the slag and the alloy were separated, and 4.64 kg of vanadium-chromium-tin-aluminum intermediate alloy with complete crystallization, no pores, and no slag inclusions was obtained.

[0049] The alloy is refined, sandblasted, crushed, screened, and manually sorted and packaged to obtain the AlV55 alloy product.

[0050] The composition of the vanadium-chromium-tin-aluminum master alloy sampled and tested was: V=65.2%, Cr=14.5%, Sn=13.7%, C=0.03%, O=0.03%, N=0.02%, and Al balance.

[0051] Embodiment 2: See also Figure 1 , Figure 2 and Figure 3 , select 5kg of 99.5% powdered vanadium pentoxide (particle size ≤ 1mm), 0.805kg of 99.5% purity SnO2, 1.02kg of 99.0% purity Cr2O3, 3.25kg of 99.5% purity aluminum particles (particle size ≤ 2mm), and 1.2kg of lime for slag making. After accurately adding, mix them thoroughly and evenly in a mixer.

[0052] according to Figure 3 It is required to prepare the smelting furnace and keep it dry.

[0053] The prepared charge was placed in the smelting furnace, the ignition agent was arranged, and the smelting was ignited. The reaction time was about 30 seconds. After standing and cooling naturally for 24 hours, the furnace was dismantled, the slag and the alloy were separated, and 4.51 kg of vanadium-chromium-tin-aluminum intermediate alloy with complete crystallization, no pores, and no slag inclusions was obtained.

[0054] The alloy is refined, sandblasted, crushed, screened, and manually sorted and packaged to obtain the AlV55 alloy product.

[0055] The composition of the vanadium-chromium-tin-aluminum master alloy sampled and tested was: V=64.7%, Cr=14.91%, Sn=14.15%, C=0.02%, O=0.07%, N=0.035Al remainder.

[0056] Compared with the prior art CN 101519743A which proposes a vanadium-chromium-aluminum alloy, in which the weight percentages of V, Cr and A1 are 23.91-44.57%, 9.00-25.71% and 37.53-56.00% respectively, and the remainder is inevitable impurities, it can be clearly seen that the vanadium content is greatly increased in the vanadium-chromium-tin-aluminum intermediate alloy produced by the present invention. When the vanadium content is increased, the yield strength, hardness, tensile strength and fatigue resistance of the alloy are enhanced, and the alloy can be better applied in the smelting market of TB5 titanium alloy.

[0057] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0058] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0059] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for producing a vanadium-chromium-tin-aluminum master alloy, characterized in that: The following steps are involved: S1. Mix V2O5, SnO2, Cr2O3, aluminum powder and slag-forming agent to obtain a charge; S2. The charge is added to the smelting furnace, the ignition agent is laid and ignited to obtain separated slag and liquid alloy; S3. After cooling, the slag is cleaned, the solidified alloy liquid is removed, impurities on the surface of the alloy liquid are cleaned and sandblasted to obtain an alloy block; S4. Crushing and screening the alloy block to obtain a vanadium-chromium-tin-aluminum master alloy.

2. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S1, the V2O5 grade is ≥99.0%, the SnO2 grade is ≥99.0%, the Cr2O3 grade is ≥99.0%, and the aluminum powder purity is ≥99.7%.

3. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S1, the block size of V2O5 is ≤3mm, the particle size of SnO2 is ≤1mm, the particle size of Cr2O3 is ≤1mm, and the particle size of aluminum powder is ≤2mm.

4. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S2, the alloy liquid is deposited at the bottom of the smelting furnace, and the slag floats on the alloy liquid.

5. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S3, the cooling requires the smelting furnace to cool for 48 hours, and the temperature inside the furnace is less than 50°C.

6. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S4, the step of crushing and screening the alloy block to obtain the vanadium-chromium-tin-aluminum master alloy comprises: Crushing and screening the alloy block to obtain alloy particles of required particle size; Through manual or machine sorting, alloy particles with oxide film are removed; The qualified alloy particles are packed in barrels and sealed to obtain vanadium-chromium-tin-aluminum master alloy.

7. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S2, the step of adding the charge into the smelting furnace and laying and igniting the ignition agent comprises: Add the prepared charge into the smelting furnace and arrange it evenly; Spread the ignition material evenly on the surface of the charge; The ignition charge is ignited.

8. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: In step S3, the step of cleaning impurities on the surface of the alloy liquid and sandblasting includes: Clean impurities on the surface of alloy liquid; Remove the defective parts of surface slag inclusions; Clean the oxidized surface by sandblasting; After sandblasting, the surface is inspected to ensure that the desired surface roughness requirements are met.

9. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: The smelting furnace uses a split graphite crucible.

10. The method for producing vanadium-chromium-tin-aluminum master alloy according to claim 1, characterized in that: The smelting furnace is composed of a furnace bottom (2) and a plurality of combinable furnace bodies (1); the plurality of combinable furnace bodies (1) and / or the furnace bottom (2) are connected using bolts or snaps.