A hot-rolled composite phase 1770MPa grade prestressed stranded wire rod and its manufacturing method
Through low-carbon and low-manganese C-Si-Mn-Cr chemical composition and online molten salt micro-quenching tempering technology, high-strength and high-plastic tempered pearlite and bainite tissues are formed, and the high-cold extraction in the existing technology is solved. The high risk of wire breaking and high material cost under the surface reduction rate have achieved efficient manufacturing of 1770MPa-level prestressed stranded wire.
Patent Information
- Application Number
- CN202411356388.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The existing hot-rolled strips for prestressed steel strands for 1770MPa grade are difficult to achieve high strength and plastic matching under high cold drawing and reduction ratio, resulting in high risk of wire breaking, high material cost, and large fluctuations in tissue uniformity and performance.
Using low-carbon and low-manganese C-Si-Mn-Cr chemical composition design, combined with online molten salt microquenching and tempering technology, it enters the bainite phase region by rapidly cooling and undergoes isothermal phase transformation in the pearlite phase region to form The structures mainly tempered pearlite and tempered bainite regulate carbide spheroidization and improve the strength and plasticity of the material.
It achieves high strength and plastic matching of the strip, reduces the risk of wire breaking, reduces material costs, and improves tissue uniformity and mechanical properties stability. It is suitable for the manufacture of high-strength 1770MPa-level prestressed strands.
Smart Images

Figure CN118895460B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of hot-rolled wire rods for stranded wires, and in particular relates to a hot-rolled complex-phase 1770MPa-grade wire rod for prestressed stranded wires and a manufacturing method thereof. Background Art
[0002] Prestressed steel strands are made by cold drawing the parent material wire rod into wire, and then twisting the wire into multiple strands. Since it is cold drawn with a large reduction rate, the reduction rate can be as high as 90%, so it has the characteristics of ultra-high strength and is widely used in high-strength anchoring fields such as construction, transportation, and machinery. At present, 1770MPa grade prestressed steel strands are usually cold drawn with 13~15mm specification wire rods as the parent material. The strength level of prestressed steel strands is determined by the strength of its parent material wire rod and the cold drawing reduction rate, that is, the parent material strength combined with the cold drawing strength increment. The lower the parent material strength, the greater the cold drawing reduction rate is required to make the steel strand reach the corresponding strength grade. The greater the cold drawing reduction rate, the higher the risk of wire breakage during the drawing and wire making process. Therefore, it is necessary to develop hot-rolled wire rods with better strength and plasticity to meet the stable drawing and twisting requirements of manufacturing 1770MPa grade prestressed steel strands under large cold drawing reduction rates.
[0003] At present, the hot-rolled wire rod for 1770MPa grade stranded wire generally adopts 82B material as raw material. In order to further improve the strength and hardenability of the wire rod, elements such as Cr and V are added to the composition, and pearlite steel is obtained by combining the post-rolling Stelmor controlled cooling line. For example, the Φ14mm high-strength wire rod for 1770MPa prestressed steel strand disclosed in patent CN104805363A and its production method adopt C-Si-Mn-Cr-V composition design, combined with rolling cooling to obtain a wire rod with an average tensile strength of 1241MPa and a cross-sectional shrinkage rate of 33%. Therefore, the following technical difficulties are still present in the manufacture of hot-rolled wire rods with finer diameter, lower cost, high strength and plasticity matching, and better uniformity of organization:
[0004] 1. Microalloy V can strengthen and toughen the matrix through fine grains, but as a precious metal, it also increases the material cost. For the purpose of reducing costs, omitting V alloy will bring about a certain strength loss; for 82B wire rod, in order to improve the strength and hardenability of the wire rod, the proportion of cementite strength phase will be increased by increasing the carbon content. The C and Mn contents are relatively high and contain Cr, but the central segregation control of the continuous casting billet is unstable. Segregation will aggravate the tendency of abnormal organization precipitation and strength fluctuation of the wire rod during the Stelmor air cooling control cooling process, resulting in the deterioration of the uniformity and plasticity of the wire rod organization. For the purpose of reducing the difficulty of organization control and performance fluctuation, reducing the C and Mn contents will also bring about a large strength loss. If the strength loss of the wire rod is too large, it is necessary to increase the cold drawing reduction rate. The plasticity loss is greater during the process, which will increase the risk of wire breakage.
[0005] Second, with the increase of carbon content and the intensification of central segregation, a large number of network cementite will be easily formed during the Stelmor controlled cooling process, which will destroy the continuity of the matrix organization, cause the decline of mechanical properties, and especially deteriorate the cold processing plasticity of the wire rod. Therefore, in order to minimize the level of network cementite and refine the interlamellar spacing of the organization to obtain the strengthened troostite organization, the prior art will use a faster roller speed and a large fan air volume to cool the wire rod after spinning. However, on the one hand, the maximum cooling rate of the wire rod is about 10℃ / s. After the secondary cementite and tertiary cementite, the wire rod will be cooled to a temperature of 10℃ / s. The time of cementite precipitation temperature range is still relatively long, and the network carbide cannot be stably avoided and the cementite coarsening will reduce the strengthening effect of carbon element. On the other hand, strong wind cooling will further increase the temperature difference between the windward side and the leeward side, and between the overlap and non-overlap due to the uncontrollable air volume, wind direction and wind temperature. Combined with the influence of high hardenability and segregation, it is easy to form abnormal bainite or martensite structure exceeding the standard in the organization, causing the wire rod to be brittle, performance fluctuations to increase, and even break during the winding process, which in turn affects the yield rate and performance of the stranded wire manufactured by downstream users.
[0006] 3. Cr can improve the hardenability of steel and the stability of supercooled austenite, so that supercooled austenite passes through the high-temperature phase transformation zone and undergoes organizational transformation at a relatively low temperature. In the process of continuous controlled cooling in Stelmor, a pearlite-based organization is formed, in which the pearlite phase is used as the strength phase and the ferrite is used as the plastic phase. The strength of the wire rod is improved by increasing the proportion of the pearlite phase. However, on the one hand, in the continuous cooling process, even if the cooling rate is reduced or the insulation cooling is performed, the time for the wire rod to pass through the pearlite phase zone is still relatively short. If the proportion of the formed pearlite organization is insufficient, it will bring about obvious strength loss. Increasing the proportion of the strength phase will reduce the proportion of the plastic phase and the strength of the wire rod will be reduced. The plasticity of the wire rod is reduced, so it is difficult to effectively improve the strength and plasticity of the wire rod by adjusting the proportion of pearlite and ferrite. On the other hand, in the early stage of controlled cooling, the large-sized cementite particles increase due to insufficient cooling rate, and the high Mn content reduces the diffusion activity of carbon, which increases the difficulty of microstructure softening. At the same time, in the continuous cooling process, the pearlite peak precipitation temperature of the stranded wire rod is low, the time through the high temperature section is short, and the temperature of the wire rod after the pearlite phase transformation is already low, the thermal power is insufficient, the matrix cannot be softened, and the microstructure dislocation is large, resulting in insufficient plasticity of the final wire rod and obvious drawing hardening, which leads to frequent wire breakage under large cold drawing reduction processing. Summary of the invention
[0007] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a hot-rolled complex phase 1770MPa grade prestressed stranded wire rod and a manufacturing method thereof, which can combine low-carbon and low-manganese components and complex phase structure regulation to reduce material costs, achieve high strength and plasticity matching of the wire rod, improve structure uniformity, and be used to manufacture 1770MPa grade prestressed stranded wire, effectively reducing the risk of wire breakage.
[0008] The technical solution adopted by the present invention to solve its technical problem is:
[0009] A method for manufacturing a hot-rolled multi-phase 1770MPa grade prestressed stranded wire rod, the manufacturing method comprising:
[0010] The wire rod is rolled according to the chemical composition of the stranded wire rod, and the chemical composition and mass percentage of the stranded wire rod include: C: 0.69%~0.74%, Si: 0.20%~0.35%, Mn: 0.10%~0.30%, Cr: 0.18%~0.30%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; after the wire rod is spun into a wire rod at a spinning temperature of ≥925°C, it is first subjected to an online molten salt micro-quenching treatment to make the wire rod cool at a cooling rate of ≥39°C / s The wire rod is cooled to enter the bainite phase region to promote the transformation of part of austenite to bainite. After that, it is treated with online molten salt tempering to heat the wire rod to the pearlite phase region for isothermal phase transformation, which promotes the transformation of untransformed austenite to pearlite. The bainite and pearlite structures are tempered and softened, and the carbides are spheroidized. Finally, it is roller cooled to produce a wire rod for stranding with a microstructure including 71% to 77% tempered pearlite by volume, 17% to 23% tempered bainite by volume, and the rest is a mixed structure composed of tempered ferrite and micro-spheroidized carbides.
[0011] The design basis of chemical composition and mass percentage of wire rod for stranding includes:
[0012] (1) Carbon: Carbon is a basic strengthening element in carbon steel and is relatively cheap. As the carbon content increases, the strength phase ratio of cementite materials will increase, and the yield strength and tensile strength of the materials will be improved. However, excessive carbon will promote central segregation during continuous casting, increase the precipitation of pro-eutectoid cementite during wire rod controlled cooling, and form a tendency of network cementite. Therefore, in order to take into account the high strength performance of 1770MPa grade stranded wire and make it easier to control the wire rod structure, the carbon content is appropriately reduced to reduce the degree of central segregation. When the wire rod is subjected to online molten salt micro-quenching treatment after spinning, ultra-fast cooling is used to further avoid the precipitation of network carbides, refine cementite carbides, reduce the difficulty of micro-spheroidization of the structure, and reduce segregation. The peak precipitation temperature of bainite and pearlite is regulated to make the bainite phase change more controllable, creating favorable conditions for the pearlite phase change while the phase temperature is relatively high and can provide more thermal power. Therefore, the mass percentage of C is controlled to be 0.69%~0.74%.
[0013] (2) Silicon: Si is often used as a deoxidizer during smelting. At the same time, as a ferrite strengthening element, it can improve the strength of ferrite through solid solution strengthening, increase the activity of carbon, accelerate the diffusion of carbon, and thus reduce the difficulty of micro-spheroidization of the organization. It is beneficial to the tempering softening of bainite and pearlite organizations and the spheroidization of carbides. It is cheaper than the Mo component that can also refine carbides. However, too much silicon will increase the graphitization tendency of C, which is not conducive to organizational uniformity and cold working performance. Therefore, in order to take into account the high strength and plasticity of the steel wire rod for stranding and facilitate the regulation of the wire rod organization, the mass percentage of Si is controlled to be 0.20%~0.35%.
[0014] (3) Manganese: As a deoxidizing element in the steelmaking process, Mn can reduce hot brittleness to ensure the smooth progress of the rolling process. At the same time, as an austenite stabilizing element, it can reduce the lower critical point of steel, reduce the phase transition temperature, refine the pearlite structure, and use solid solution strengthening to increase the strength, wear resistance and hardenability of the wire rod. However, when the Mn content is too high, it is easy to segregate in the steel, slow down the diffusion rate of C, significantly increase the hardenability of the wire rod core, and expand the bainite and martensite phase transition temperature range. It is not conducive to the control of bainite phase transformation in online molten salt micro-quenching treatment, making it easier for martensite to appear in the core and reduce the drawing performance of the wire rod. Excessive Mn content will also increase material costs. Therefore, in order to take into account the high strength and toughness of the steel wire rod for stranding and facilitate the uniformity of the wire rod structure, the Mn content is appropriately reduced, and the mass percentage of Mn is controlled to be 0.10%~0.30%.
[0015] (4) Chromium: Cr is a medium-strong carbide-forming element commonly used in high carbon steel. It can improve the stability and hardenability of austenite, inhibit the precipitation of proeutectoid ferrite, prevent the growth of grains during hot rolling, delay the nucleation and growth of carbides, refine the structure, refine the pearlite interlamellar spacing, and reduce the difficulty of tempering and spheroidization. After online molten salt tempering treatment, it can form a dispersed carbide-reinforced matrix, thereby improving the strength and wear resistance of the wire rod. However, too high Cr content will aggravate the segregation of central alloy elements, slow down the diffusion of carbon, and affect the peak precipitation temperature of pearlite. There is a risk of coarse grains under long-term online molten salt tempering treatment, which is not conducive to structure control and will increase manufacturing costs. Therefore, the mass percentage of Cr is controlled to be 0.18%~0.30%.
[0016] (5) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0017] The above-mentioned stranded wire rod adopts a low-carbon and low-manganese C-Si-Mn-Cr composition design, without adding micro-alloy elements such as V, which can reduce material costs, reduce segregation tendency, adjust the CCT curve to move upward, and narrow the bainite phase transformation temperature range. Combined with online molten salt quenching + tempering treatment directly after spinning:
[0018] 1. Compared with the existing Stelmor strong air cooling process after spinning, online molten salt micro-quenching can utilize the high heat exchange capacity of molten salt to cool the wire rod more quickly, effectively reducing the time passing through the temperature range of secondary cementite precipitation, avoiding the formation of network carbides and deteriorating the uniformity and plasticity of the organization, while inhibiting the large-scale precipitation of tertiary cementite, refining cementite carbides, and improving the strengthening effect of carbon elements to compensate for the strength loss caused by reducing carbon content.
[0019] 2. Compared with the existing air cooling process after spinning, in which the precipitation of abnormal tissue is uncontrollable, online molten salt quenching can utilize the rapid cooling of the wire rod, which is more conducive to the refinement of cementite carbides, and also allows the wire rod to quickly enter the bainite phase region with a lower temperature than the pearlite phase region from the high-temperature austenite state. Micro-quenching is performed first to increase the nucleation driving force, control the partial austenite phase transformation to high-strength bainite structure with fine grain size. At the same time, since the molten salt is wrapped on the surface of the wire rod, the heat transfer is rapid and more uniform, and there is no temperature difference problem between the windward side and the leeward side. Combined with the decrease in the tendency of component segregation, it can also avoid the wire rod from entering the martensite phase region. The formation of abnormal martensite structure, thereby making the proportion of tempered bainite in the structure controllable.
[0020] 3. Compared with the existing continuous controlled cooling after spinning, it is difficult to take into account both the strength and plasticity of the wire rod. On the one hand, the wire rod is subjected to online molten salt micro-quenching treatment to form a small amount of bainite. After being heated to the pearlite phase region through online molten salt tempering, the wire rod temperature can be kept consistent with the molten salt temperature. Compared with continuous cooling, the wire rod stays in the pearlite phase region for a longer time, which can control the untransformed high-temperature austenite to transform into full pearlite, forming a structure dominated by pearlite and bainite, reducing the proportion of ferrite, and having a higher matrix strength than the pearlite + ferrite wire rod structure, which can make up for the strength loss caused by reducing the C and Mn content and not adding the V element. On the other hand, the temperature of the pearlite phase region is higher than that of the troostite and bainite phase regions, which can control the wire rod. When isothermal, it is in a high temperature state for a longer time, which increases the thermal power, promotes further tempering and softening of bainite and pearlite structures formed by phase transformation, and transforms carbides into spheroidized structures. Cr carbides are dispersed in the plastic matrix to reduce tissue stress and dislocation density. Compared with the existing practice of regarding bainite as a brittle abnormal structure, the strength characteristics of bainite can be well utilized to obtain a tempered bainite structure that is both strong and tough. The plasticity of the pearlite structure is improved, and then roller cooling is performed. The high temperature state of the wire rod after leaving the salt bath can be utilized to continue the tempering and softening effect of the later stage of online molten salt tempering, promote further spheroidization of carbides, and improve the plasticity of the material, and finally achieve tissue regulation, high strength and plasticity matching, and effectively improve the uniformity of the structure.
[0021] A higher heating furnace temperature and a shorter furnace time are selected before rolling to promote uniform composition of the continuous casting billet and reduce the degree of decarburization of the billet. In a preferred embodiment, before rolling, the heating furnace temperature is controlled to be ≤1120°C and the furnace time is ≤3h.
[0022] Since the spinning temperature is relatively high, a higher rolling temperature can be used to increase the rolling speed and efficiency, reduce the deformation resistance of the rolled piece, and facilitate the implementation of controlled rolling. At the same time, a larger rolling reduction is used to promote grain refinement. The final rolling stage promotes austenite recrystallization and improves the strength and toughness of the matrix. In a preferred embodiment, during the rolling, the initial rolling temperature is controlled to be 1060~1100℃, the initial rolling reduction is 25%~35%, the final rolling temperature is ≤955℃, and the final rolling reduction is 28%~38%.
[0023] In a preferred embodiment, the molten salt temperature of the online molten salt micro-quenching treatment is 430-478°C, and the treatment time is 20-40s. The molten salt temperature is in the higher temperature section of the bainite phase region. The lower the molten salt temperature of the online molten salt micro-quenching treatment and the longer the treatment time, the more austenite is transformed into bainite, the proportion of tempered bainite increases, the strength of the wire rod increases, and the plasticity decreases. However, if the molten salt temperature is too low and the treatment time is too long, too much bainite structure or even martensite structure will be produced, which will affect the formation of most tempered bainite. The high plasticity of pearlite and regulating wire rod is not favorable; on the contrary, the higher the molten salt temperature and the shorter the treatment time of the online molten salt micro-quenching treatment, the lower the proportion of tempered bainite, the lower the strength of the wire rod and the higher the plasticity. However, the molten salt temperature is too high and the treatment time is too short, which is in the troostite phase region, which is not conducive to the formation of a small amount of bainite and then tempering to provide matrix strength. Therefore, the molten salt temperature and treatment time of the online molten salt micro-quenching treatment can be controlled to control the formation of bainite, so as to make organizational preparations for organizational tempering and regulating the proportion of tempered pearlite.
[0024] Since the temperature difference of the wire rod from the spinning temperature to the bainite phase temperature is large, selecting a larger molten salt circulation rate can control the molten salt temperature rise, improve the accuracy of micro-quenching treatment, and control the bainite phase transformation through short-time treatment. In a preferred embodiment, the molten salt circulation rate of the online molten salt micro-quenching treatment is 450~550t / h, and the molten salt temperature rise is ≤10℃.
[0025] In a preferred embodiment, the molten salt temperature of the online molten salt tempering treatment is 530~570℃, and the treatment time is 300~550s. This molten salt temperature is in the lower temperature range of the pearlite phase region. The lower the molten salt temperature, the finer the pearlite lamellae spacing formed. As the treatment time increases, the proportion of pearlite with fine lamellae spacing increases and the proportion of ferrite decreases. However, if the molten salt temperature is too low, it is difficult to form a large thermal dynamic force, which is not conducive to the tempering softening of bainite and pearlite structures, and will cause the plasticity of the matrix to decrease. On the contrary, if the molten salt temperature is higher, the coarser the pearlite lamellae formed, which is beneficial to the spheroidization and softening of the structure, and can improve the spheroidization level of carbides, reduce the strength of the wire rod and increase the plasticity. However, if the molten salt temperature is too high, the pearlite lamellae are too coarse, the pearlite nucleation rate decreases, which is not conducive to reducing the proportion of tempered ferrite, and the structure is too softened or softened too quickly, which affects the strength and stability of the matrix. It is unfavorable, and it will also cause the online time of roller cooling to be extended, which is not conducive to optimizing production efficiency; the longer the treatment time, the better the tempering and softening effect of bainite and pearlite, the matrix strength decreases and the plasticity increases, but if the treatment time is too long, the production energy consumption increases, and there is also the risk of Cr precipitation coarsening and micro-spheroidized carbides growing together and losing strength and plasticity; on the contrary, the shorter the treatment time, the lower the softening effect and the plasticity of the wire rod, but if the treatment time is too short, the bainite fails to soften, which will bring greater brittleness, the untransformed high-temperature austenite fails to fully transform into pearlite structure, and the austenite residue has the risk of forming abnormal structure during roller cooling, which is not conducive to the regulation of matrix plasticity and uniformity. Therefore, the molten salt temperature and treatment time of online molten salt tempering treatment can be further controlled to promote sufficient pearlite phase transformation and appropriate tempering regulation, and further regulate the strength and plasticity of the wire rod.
[0026] Since the temperature difference of the molten salt in the online molten salt micro-quenching and online molten salt tempering stages is relatively small, a relatively small molten salt circulation amount can be selected to control the molten salt temperature rise, improve the tempering treatment accuracy, and reduce the tempering treatment energy consumption. In a preferred embodiment, the molten salt circulation amount of the online molten salt tempering treatment is 150~350t / h, and the molten salt temperature rise is ≤5°C.
[0027] Since the molten salt temperature of the online molten salt tempering treatment is relatively high, controlling the cooling rate of the roller cooling can promote further softening of the wire rod and avoid loss of wire rod strength due to too low cooling rate and affecting efficient production due to low roller speed. In a preferred embodiment, the roller cooling controls the wire rod to slowly cool at a cooling rate of 0.65~0.85℃ / s until it is coiled.
[0028] In a preferred embodiment, the roller cooling adopts a closed insulation cover, and the wire rod is transported at a roller speed of 0.1~0.3m / s in the insulation cover. The waste heat of the wire rod itself can be radiated into the insulation cover to form an insulation cooling environment. The cooling speed of the wire rod can be further controlled by adjusting the appropriate roller speed, and the energy consumption is relatively small.
[0029] In a preferred embodiment, after coiling, the wire rod is controlled to be gradually cooled to room temperature at a cooling rate of ≤2°C / s, so as to avoid loss of wire rod plasticity due to excessive cooling speed and further control the stability of the same circle size.
[0030] In a preferred embodiment, the coils are piled up to cool in a wind-proof manner after being assembled, and the residual heat of the coils can be used to avoid excessively fast cooling.
[0031] A hot-rolled complex phase 1770 MPa grade prestressed stranded wire rod, the stranded wire rod is manufactured by any of the above-mentioned methods for manufacturing the hot-rolled complex phase 1770 MPa grade prestressed stranded wire rod.
[0032] The above-mentioned stranded wire rod adopts the C-Si-Mn-Cr chemical composition, which is a low-carbon, low-manganese, and vanadium-free composition design, and has lower material cost. The formed microstructure includes most tempered pearlite, a small part of tempered bainite, and a small amount of tempered ferrite and micro-spheroidized carbides. Compared with the existing pearlite / sorbite + ferrite stranded wire rod structure, the tempered pearlite can retain the characteristics of moderate strength and plasticity, such as coarser pearlite interlamellar spacing than sorbite interlamellar spacing, better plasticity than sorbite, and higher strength than ferrite. After tempering, the organizational stress and dislocation density decrease, which can greatly improve the cold drawing performance and avoid drawing hardening. The tempered bainite utilizes the high strength characteristics of the brittle phase of bainite and undergoes tempering transformation. The invention has a strong and tough organizational state, in which the proportion of tempered bainite is controllable and abnormal martensite organization can be avoided, so a organization mainly composed of tempered pearlite and tempered bainite is formed. Unlike increasing the soft-phase ferrite in the organization to improve the toughness of the steel but excessively losing the strength of the wire rod, the present invention can reduce the proportion of tempered ferrite, and provide a higher matrix strength in combination with a small amount of tempered bainite, to make up for the strength loss caused by reducing the C and Mn contents and eliminating the V element. On the basis of not excessively deteriorating the strength of the wire rod, the spheroidization of carbides and the tempering of the organization are used to greatly improve the matrix plasticity, thereby taking into account the high strength and higher plasticity matching of the wire rod, which is beneficial to reduce the risk of wire breakage during the cold drawing and multi-strand twisting process of the prestressed stranded wire with a large area reduction rate.
[0033] In a preferred embodiment, the spacing between the tempered pearlite lamellae of the stranded wire rod is 160-210 nm, the tempered pearlite lamellae are relatively small, and the stress concentration caused by plastic deformation is reduced, which is beneficial to improving the strength of the wire rod.
[0034] In a preferred embodiment, the network carbide level of the stranded wire rod is level 0, which can avoid the adverse effects of the network carbide on the plasticity and organizational uniformity of the wire rod and improve the utilization value and strengthening effect of the carbon element.
[0035] Since the wire rod has no network carbide and abnormal martensite structure, and the uniformity of the structure is improved after the phase transformation, the fluctuation of the mechanical properties is correspondingly reduced. In a preferred embodiment, the same-turn difference of the mechanical properties of the wire rod for stranding is ≤24MPa.
[0036] In a preferred embodiment, the diameter of the wire rod for the stranded wire is 8.0~13.0mm, the tensile strength is 1185~1215MPa, and the cross-sectional shrinkage rate is 40%~45%. The wire rod has a smaller initial diameter, which can reduce the number of drawing passes during prestressed stranded wire making, quickly reach the target diameter, and improve production efficiency. At the same time, the wire rod has a higher tensile strength and significantly improved cross-sectional shrinkage rate. It can be processed into 1770MPa grade prestressed steel strands through pickling, drawing, and twisting, which is beneficial to hinder crack propagation, thereby reducing the wire breakage rate and improving the yield rate of stranded wire.
[0037] Compared with the prior art, the beneficial effects of the present invention are at least:
[0038] (1) In view of the current situation that the uniformity of wire rod structure and high-strength and plastic properties are difficult to control in the production of existing 1770MPa grade prestressed steel strands due to the insufficient cooling capacity of the Stelmor air-cooling line, the present invention adopts a low-carbon and low-manganese C-Si-Mn-Cr chemical composition design combined with an online molten salt micro-quenching + tempering technology process design, and utilizes the high-speed heat exchange capacity of the molten salt to control the fast wire rod to enter the bainite phase region for micro-quenching treatment, which can avoid network carbides and inhibit the precipitation of tertiary cementite. Combined with the strengthening effect of a small amount of bainite phase transformation, the strengthening effect of the carbon element is maximized to compensate for the strength loss caused by reducing the C and Mn content and eliminating the V element. Then, through online molten salt tempering, the untransformed high-temperature austenite is controlled to enter the pearlite phase region for isothermal phase transformation, and at the same time, the bainite and pearlite structures formed by the phase transformation are further tempered and softened to improve the plasticity of the material, achieve high strength and plasticity matching of the wire rod, improve the uniformity of the structure, and have good industrial adaptability.
[0039] (2) In view of the fact that the existing 1770MPa grade prestressed steel strand wire rod material cost is relatively high, and the risk of wire rod breaking during the drawing and wire making process is high due to the large cold drawing area reduction rate and insufficient plasticity, the wire rod for strand wire of the present invention is designed with low carbon, low manganese and vanadium-free components, which can reduce material costs. The microstructure type is a mixed structure composed of tempered pearlite with higher plasticity, tempered bainite with both strength and toughness, tempered ferrite with a smaller proportion, and micro-spheroidized carbides, and does not contain abnormal martensitic structure, which can achieve high strength and plasticity matching of the wire rod. The wire rod diameter specification can be made finer, reaching a tensile strength of 1185~1215MPa and a cross-sectional shrinkage rate of 40%~45%. It is used in the manufacture of 1770MPa grade prestressed strand wire and other application fields, which is beneficial to meeting the requirements of large cold drawing area reduction rate and rapid wire making, reducing the risk of wire breaking during drawing and wire making, and thus improving the processing efficiency and yield rate of prestressed strand wire, and has good market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0041] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0042] Figure 2 It is the metallographic structure diagram of Example 2 of the present invention. DETAILED DESCRIPTION
[0043] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention, so as to propose the best way to implement the present invention, and are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention, but cannot be understood as any limitation on the scope of the present invention, which is limited only by the appended claims; the organization and performance testing of the wire rods obtained in the following embodiments and comparative examples include: the tensile test is carried out using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain the tensile strength and cross-sectional shrinkage rate, and the organization test is carried out according to the metal microstructure detection method of GB / T13298 standard; the mechanical property same circle difference test method: take 2 circles of wire rod 5m away from the end of the coil, take the overlap area position as the base point, divide each circle of wire rod into 8 sections on average, take 1 tensile specimen on each section, and the strength extreme difference of the tensile specimen after the tensile test is the mechanical property same circle difference. Embodiment 1:
[0044] A preferred embodiment of the method for manufacturing the hot-rolled complex phase 1770MPa grade prestressed stranded wire rod of the present invention, the chemical composition and mass percentage of the stranded wire rod include: C: 0.72%, Si: 0.2%, Mn: 0.1%, Cr: 0.3%, P: 0.012%, S: 0.013%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of rolling → spinning → online molten salt micro-quenching + tempering → roller cooling → coiling, specifically:
[0045] The rolling process is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity, promote the uniformity of the steel billet composition and reduce the degree of decarburization of the steel billet, and then roll the steel billet into a wire with a diameter of 8mm through a rolling line, improve the rolling efficiency with a higher rolling temperature, and promote grain refinement with a larger rolling reduction, specifically: control the heating furnace temperature ≤1080℃, the furnace time is 2.5h, the initial rolling temperature is 1060℃, the initial rolling reduction is 35%, the final rolling temperature is 935℃, and the final rolling reduction is 38%; the wire-spinning process is used to convert the wire exiting the rolling line into a wire rod through a wire-spinning mechanism, and the wire rod is spread on the roller and transported along the roller to avoid the network carbide caused by too low a wire-spinning temperature, specifically: control the wire-spinning temperature to 925℃.
[0046] The online molten salt micro-quenching + tempering process adopts two salt baths with molten salt inside. The wire rod after spinning is conveyed by rollers through the first salt bath, and is quickly cooled to the molten salt temperature for online molten salt micro-quenching treatment, so that the wire rod is cooled at a cooling rate of 39°C / s until it enters the bainite phase region, avoiding the precipitation of secondary cementite, inhibiting the peak precipitation of tertiary cementite, refining cementite carbides, and promoting the transformation of part of high-temperature austenite to bainite. After that, the wire rod is conveyed by rollers through the second salt bath, so that the wire rod is heated to the pearlite phase region for isothermal phase transformation, that is, online molten salt micro-quenching + tempering process. Salt tempering treatment promotes the transformation of high-temperature austenite that has not been transformed during micro-quenching to pearlite. With the long-term isothermal tempering, the formed bainite and pearlite structures are tempered and softened, and the carbides are spheroidized, so as to adjust the strength and plasticity matching of the wire rod. Specifically: the molten salt temperature of the online molten salt micro-quenching treatment is 478°C, the treatment time is 20s, the molten salt circulation volume is 450t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the online molten salt tempering treatment is 570°C, the treatment time is 550s, the molten salt circulation volume is 200t / h, and the molten salt temperature rise is ≤5°C.
[0047] The roller cooling process is closed with a heat preservation cover, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the heat preservation cover for cooling treatment to promote further tempering, softening and spheroidization of the structure. Specifically: the wire rod is conveyed at a roller speed of 0.3m / s in the heat preservation cover, and the wire rod is controlled to be slowly cooled at a cooling rate of 0.85℃ / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 300℃. After coiling, the coil is piled up to avoid wind and cooled, and the coil is controlled to be gradually cooled to room temperature at a cooling rate of ≤2℃ / s. After packaging and storage, the hot-rolled wire rod product is obtained, and its metallographic structure diagram is as follows Figure 1 As shown, the microstructure is 71% by volume of tempered pearlite + 17% by volume of tempered bainite + 5% by volume of tempered ferrite + 7% by volume of micro-spheroidized carbide, the interlamellar spacing of tempered pearlite is 210nm, the grade of network carbide is 0, the difference in mechanical properties is 20MPa, the tensile strength is 1185MPa, and the section reduction rate is 45%.
[0048] Comparative Example 1:
[0049] A method for manufacturing a hot-rolled wire rod, the manufacturing method of which is different from that of Example 1 in that: the manufacturing method is manufactured according to the process flow of rolling → spinning → Stelmor strong air cooling → roller cooling, specifically: the heating furnace temperature is controlled to be ≤1050°C, the furnace time is 3h, the initial rolling temperature is 1015°C, the final rolling temperature is 885°C, and the spinning temperature is 865°C; the Stelmor strong air cooling uses an air volume of 200,000 m per fan 3 / h, 1~7# fans are opened at 90%, and the wire rod is controlled to be cooled to 640℃ at 8.5℃ / s. The roller cooling adopts closing the fan, and the wire rod is conveyed at a roller speed of 0.15m / s. The wire rod is controlled to be cooled to 300℃ at a cooling rate of 1.5℃ / s. After going off the line, the wire rod is controlled to be pile-cooled in a wind-proof manner to obtain a finished wire rod, the microstructure of which is 85% pearlite by volume + 15% ferrite by volume, the pearlite lamellar spacing is 251nm, the network carbide grade is 1, the mechanical property same circle difference is 54MPa, the tensile strength is 1080MPa, and the cross-sectional shrinkage rate is 30%.
[0050] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with Stelmor air cooling, the cooling capacity is limited, the level of network carbides is higher, the strength loss of the obtained pearlite + ferrite structure is large, the plasticity is insufficient, and the mechanical properties fluctuate greatly. The present invention combines low-carbon and low-manganese components with complex phase structure regulation, utilizes the high-speed heat exchange capacity of molten salt, and controls the fast wire rod to enter the bainite phase area for micro-quenching treatment, which can avoid network carbides, inhibit the precipitation of tertiary cementite, and compensate for the strength loss caused by reducing the C and Mn content and eliminating the V element. At the same time, it promotes the further tempering and softening of the bainite and pearlite structures formed by phase transformation, which can effectively improve the plasticity of the material.
[0051] Comparative Example 2:
[0052] A method for manufacturing a hot-rolled wire rod, the manufacturing method differs from that of Example 1 in that: the heating furnace temperature is controlled to be ≤1060°C, the furnace time is 3h, the initial rolling temperature is 1040°C, the final rolling temperature is 925°C, the spinning temperature is 900°C, during online molten salt micro-quenching treatment, the wire rod is cooled at a cooling rate of 37°C / s until it enters a bainite phase region; and the finished wire rod is obtained after windproof pile cooling. Embodiment 2:
[0053] A preferred embodiment of the method for manufacturing the hot-rolled complex phase 1770MPa grade prestressed stranded wire rod of the present invention, the chemical composition and mass percentage of the stranded wire rod include: C: 0.73%, Si: 0.26%, Mn: 0.29%, Cr: 0.23%, P: 0.015%, S: 0.013%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of rolling → spinning → online molten salt micro-quenching + tempering → roller cooling → coiling, specifically:
[0054] The rolling process is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic, promote the uniformity of the steel billet composition and reduce the degree of decarburization of the steel billet, and then roll the steel billet into a wire with a diameter of 12mm through a rolling line, improve the rolling efficiency with a higher rolling temperature, and promote grain refinement with a larger rolling reduction, specifically: control the heating furnace temperature ≤1110°C, the furnace time is 3h, the initial rolling temperature is 1090°C, the initial rolling reduction is 28%, the final rolling temperature is 950°C, and the final rolling reduction is 30%; the wire-spinning process is used to convert the wire exiting the rolling line into a wire rod through a wire-spinning mechanism, and the wire rod is spread on the roller and transported along the roller to avoid the network carbide caused by too low a wire-spinning temperature, specifically: control the wire-spinning temperature to 935°C.
[0055] The online molten salt micro-quenching + tempering process adopts two salt baths with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath, and is quickly cooled to the molten salt temperature for online molten salt micro-quenching treatment, so that the wire rod is cooled at a cooling rate of 40°C / s until it enters the bainite phase region, avoiding the precipitation of secondary cementite, inhibiting the peak precipitation of tertiary cementite, refining cementite carbides, and promoting the transformation of part of high-temperature austenite to bainite. After that, the wire rod is conveyed by a roller to pass through the second salt bath, so that the wire rod is heated to the pearlite phase region for isothermal phase transformation, that is, online molten salt micro-quenching + tempering process. Salt tempering treatment promotes the transformation of high-temperature austenite that has not been transformed during micro-quenching to pearlite. With the long-term isothermal tempering, the formed bainite and pearlite structures are tempered and softened, and the carbides are spheroidized, so as to adjust the strength and plasticity matching of the wire rod. Specifically: the molten salt temperature of the online molten salt micro-quenching treatment is 452°C, the processing time is 29s, the molten salt circulation volume is 500t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the online molten salt tempering treatment is 530°C, the processing time is 390s, the molten salt circulation volume is 150t / h, and the molten salt temperature rise is ≤5°C.
[0056] The roller cooling process is closed with a heat preservation cover, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the heat preservation cover for cooling treatment to promote further tempering, softening and spheroidization of the structure. Specifically: the wire rod is conveyed at a roller speed of 0.1m / s in the heat preservation cover, and the wire rod is controlled to be slowly cooled at a cooling rate of 0.65℃ / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 284℃. After coiling, the coil is piled up to cool in a windproof manner, and the coil is controlled to be gradually cooled to room temperature at a cooling rate of ≤2℃ / s. After packaging and storage, the hot-rolled wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.
[0057] Comparative Example 3:
[0058] A method for manufacturing a hot-rolled wire rod, the manufacturing method of which differs from that of Example 2 in that: during the online molten salt micro-quenching treatment, the wire rod is cooled at a cooling rate of 39°C / s until it enters a bainite phase region, the molten salt temperature is 482°C, and the treatment time is 15s; the finished wire rod is obtained after windproof pile cooling.
[0059] Comparative Example 4:
[0060] A method for manufacturing a hot-rolled wire rod, the manufacturing method of which differs from that of Example 2 in that: during the online molten salt micro-quenching treatment, the wire rod is cooled at a cooling rate of 41°C / s until it enters a bainite phase region, the molten salt temperature is 425°C, and the treatment time is 45s; the finished wire rod is obtained after windproof pile cooling. Embodiment 3:
[0061] A preferred embodiment of the method for manufacturing the hot-rolled complex phase 1770MPa grade prestressed stranded wire rod of the present invention, the chemical composition and mass percentage of the stranded wire rod include: C: 0.69%, Si: 0.35%, Mn: 0.21%, Cr: 0.18%, P: 0.015%, S: 0.015%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of rolling → spinning → online molten salt micro-quenching + tempering → roller cooling → coiling, specifically:
[0062] The rolling process is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to obtain a high-temperature steel billet with rollable plasticity, promote uniform composition of the steel billet and reduce the degree of decarburization of the steel billet, and then roll the steel billet into a wire with a diameter of 10mm through a rolling line, improve the rolling efficiency with a higher rolling temperature, and promote grain refinement with a larger rolling reduction, specifically: control the heating furnace temperature ≤1090°C, the furnace time is 2.5h, the initial rolling temperature is 1075°C, the initial rolling reduction is 31%, the final rolling temperature is 945°C, and the final rolling reduction is 35%; the wire-spinning process is used to convert the wire exiting the rolling line into a wire rod through a wire-spinning mechanism, and the wire rod is spread on the roller and transported along the roller to avoid the network carbide caused by too low a wire-spinning temperature, specifically: control the wire-spinning temperature to 930°C.
[0063] The online molten salt micro-quenching + tempering process adopts two salt baths with molten salt inside. The wire rod after spinning is conveyed by a roller to pass through the first salt bath, and is quickly cooled to the molten salt temperature for online molten salt micro-quenching treatment, so that the wire rod is cooled at a cooling rate of 40°C / s until it enters the bainite phase region, avoiding the precipitation of secondary cementite, inhibiting the peak precipitation of tertiary cementite, refining cementite carbides, and promoting the transformation of part of high-temperature austenite to bainite. After that, the wire rod is conveyed by a roller to pass through the second salt bath, so that the wire rod is heated to the pearlite phase region for isothermal phase transformation, that is, online molten salt micro-quenching + tempering process. Salt tempering treatment promotes the transformation of high-temperature austenite that has not been transformed during micro-quenching to pearlite. With the long-term isothermal tempering, the formed bainite and pearlite structures are tempered and softened, and the carbides are spheroidized, so as to adjust the strength and plasticity matching of the wire rod. Specifically: the molten salt temperature of the online molten salt micro-quenching treatment is 445°C, the processing time is 37s, the molten salt circulation volume is 500t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the online molten salt tempering treatment is 558°C, the processing time is 485s, the molten salt circulation volume is 320t / h, and the molten salt temperature rise is ≤5°C.
[0064] The roller cooling process is closed with an insulation cover, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for cooling treatment to promote further tempering, softening and spheroidization of the structure. Specifically: the wire rod is conveyed at a roller speed of 0.25m / s in the insulation cover, and the wire rod is controlled to be slowly cooled at a cooling rate of 0.7℃ / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 330℃. After coiling, the coil is piled up to cool in a windproof manner, and the coil is controlled to be gradually cooled to room temperature at a cooling rate of ≤2℃ / s, and the hot-rolled wire rod product is obtained after packaging and storage.
[0065] Comparative Example 5:
[0066] A method for manufacturing a hot-rolled wire rod, which differs from Example 3 in that: the molten salt temperature of the online molten salt tempering treatment is 580°C, the treatment time is 600s, and the molten salt circulation rate is 400t / h; the finished wire rod is obtained after windproof pile cooling.
[0067] Comparative Example 6:
[0068] A method for manufacturing a hot-rolled wire rod, the manufacturing method of which is different from that of Example 3 in that: the molten salt temperature of the online molten salt tempering treatment is 520°C, and the treatment time is 250s; and the finished wire rod is obtained after windproof pile cooling. Embodiment 4:
[0069] A preferred embodiment of the method for manufacturing the hot-rolled complex phase 1770MPa grade prestressed stranded wire rod of the present invention, the chemical composition and mass percentage of the stranded wire rod include: C: 0.74%, Si: 0.32%, Mn: 0.3%, Cr: 0.21%, P: 0.013%, S: 0.014%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of rolling → spinning → online molten salt micro-quenching + tempering → roller cooling → coiling, specifically:
[0070] The rolling process is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic, promote the uniformity of the steel billet composition and reduce the degree of decarburization of the steel billet, and then roll the steel billet into a wire with a diameter of 13mm through a rolling line, improve the rolling efficiency with a higher rolling temperature, and promote grain refinement with a larger rolling reduction, specifically: control the heating furnace temperature ≤1120℃, the furnace time is 3h, the initial rolling temperature is 1100℃, the initial rolling reduction is 25%, the final rolling temperature is 955℃, and the final rolling reduction is 28%; the wire-spinning process is used to convert the wire exiting the rolling line into a wire rod through a wire-spinning mechanism, and the wire rod is spread on the roller and transported along the roller to avoid the network carbide caused by too low a wire-spinning temperature, specifically: control the wire-spinning temperature to 940℃.
[0071] The online molten salt micro-quenching + tempering process adopts two salt baths with molten salt inside. The wire rod after spinning is conveyed by rollers through the first salt bath, and is quickly cooled to the molten salt temperature for online molten salt micro-quenching treatment, so that the wire rod is cooled at a cooling rate of 41°C / s until it enters the bainite phase region, avoiding the precipitation of secondary cementite, inhibiting the peak precipitation of tertiary cementite, refining cementite carbides, and promoting the transformation of part of high-temperature austenite to bainite. After that, the wire rod is conveyed by rollers through the second salt bath, so that the wire rod is heated to the pearlite phase region for isothermal phase transformation, that is, online molten salt micro-quenching + tempering process. Salt tempering treatment promotes the transformation of high-temperature austenite that has not been transformed during micro-quenching to pearlite. With the long-term isothermal tempering, the formed bainite and pearlite structures are tempered and softened, and the carbides are spheroidized, so as to adjust the strength and plasticity matching of the wire rod. Specifically: the molten salt temperature of the online molten salt micro-quenching treatment is 430°C, the processing time is 40s, the molten salt circulation volume is 550t / h, and the molten salt temperature rise is ≤10°C; the molten salt temperature of the online molten salt tempering treatment is 545°C, the processing time is 300s, the molten salt circulation volume is 350t / h, and the molten salt temperature rise is ≤5°C.
[0072] The roller cooling process is closed with an insulation cover, and the wire rod coming out of the second salt bath tank is conveyed by rollers into the insulation cover for cooling treatment to promote further tempering, softening and spheroidization of the structure. Specifically: the wire rod is conveyed at a roller speed of 0.15m / s in the insulation cover, and the wire rod is controlled to be slowly cooled at a cooling rate of 0.75℃ / s until it is coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 295℃. After coiling, the coil is piled up to cool in a windproof manner, and the coil is controlled to be gradually cooled to room temperature at a cooling rate of ≤2℃ / s, and the hot-rolled wire rod product is obtained after packaging and storage.
[0073] Comparative Example 7:
[0074] A method for manufacturing hot-rolled wire rod, which differs from Example 4 in that: the roller cooling adopts a heat preservation cover to open, the wire rod is transported at a roller speed of 0.25m / s, and the wire rod is cooled to 295°C at a cooling rate of 1.3°C / s; the finished wire rod is obtained after windproof stack cooling.
[0075] The structure and performance of the wire rods obtained in the above examples 1 to 4 and comparative examples 2 to 7 were tested, and the comparative results obtained are shown in Table 1 below:
[0076] Table 1. Comparison of the microstructure and properties of different wire rod compositions and manufacturing methods
[0077]
[0078] It can be seen from the results of Examples 1 to 4 that the microstructure of the wire rod of the present invention includes a majority of tempered pearlite, a small portion of tempered bainite and a small amount of tempered ferrite and micro-spheroidized carbide, taking into account the high strength of the wire rod and a higher plasticity match, achieving a tensile strength of 1185 to 1215 MPa and a cross-sectional shrinkage rate of 40% to 45%, which is used in the manufacture of 1770 MPa-grade prestressed stranded wire and other application fields, and is beneficial to improving the processing efficiency and yield rate of prestressed stranded wire.
[0079] From the comparison results of Example 1 and Comparative Example 2, it can be seen that after lowering the spinning temperature, the rolling temperature is reduced accordingly, which is beneficial to the refinement of the grains and the toughening of the matrix, but the rolling efficiency is reduced and the rolling line load is increased. At the same time, the cooling rate of the online molten salt micro-quenching treatment is reduced accordingly, which is not conducive to the refinement of the cementite lamellae and the promotion of the tempering and softening of the bainite and pearlite structures, which will lead to the loss of strength and plasticity and the increase of mechanical property fluctuations.
[0080] It can be seen from the results of Examples 1 to 4 that the higher the molten salt temperature and the shorter the treatment time of the online molten salt micro-quenching treatment, the lower the proportion of tempered bainite, the lower the wire rod strength and the higher the plasticity. From the comparison results of Example 2 and Comparative Example 3, it can be seen that the molten salt temperature of the online molten salt micro-quenching treatment is too high and the treatment time is too short, which is not conducive to the formation of a small amount of bainite and then tempering to provide matrix strength.
[0081] It can be seen from the results of Examples 1 to 4 that the lower the molten salt temperature and the longer the treatment time of the online molten salt micro-quenching treatment, the more austenite is transformed into bainite, the proportion of tempered bainite increases, the strength of the wire rod increases, and the plasticity decreases. From the comparison results of Example 2 and Comparative Example 4, it can be seen that the molten salt temperature of the online molten salt micro-quenching treatment is too low and the treatment time is too long, resulting in excessive bainite structure, which is not conducive to regulating the high plasticity of the wire rod.
[0082] It can be seen from the results of Examples 1 to 4 that the higher the molten salt temperature and the longer the treatment time of the online molten salt tempering treatment, the more beneficial it is to the spheroidization and softening of the organization, and the spheroidization level of the carbide can be improved, the strength of the wire rod can be reduced, and the plasticity can be increased. It can be seen from the comparison results of Example 3 and Comparative Example 5 that the molten salt temperature of the online molten salt tempering treatment is too high, and a larger molten salt circulation amount is required, the production energy consumption increases, the pearlite lamellae are too coarse, the pearlite nucleation rate decreases, which is not conducive to reducing the proportion of tempered ferrite, the treatment time is too long, the production energy consumption increases, and there is also the risk of precipitation coarsening of Cr and the growth of micro-spheroidized carbides, resulting in a loss of strength and plasticity.
[0083] It can be seen from the results of Examples 1 to 4 that the lower the molten salt temperature and the shorter the treatment time of the online molten salt tempering treatment, the finer the pearlite lamella spacing formed, the reduced softening effect, and the reduced plasticity of the wire rod. It can be seen from the comparison results of Example 3 and Comparative Example 6 that the molten salt temperature and the treatment time of the online molten salt tempering treatment are too low and the treatment time is too short, and it is difficult to form a large thermal dynamic force, which is not conducive to the tempering softening of bainite and pearlite structures, and will result in insufficient plasticity of the wire rod.
[0084] From the comparison results of Example 4 and Comparative Example 7, it can be seen that reducing the cooling rate of the wire rod during the roller cooling process can continue the tempering softening effect in the later stage of online molten salt tempering, promote further spheroidization of carbides, and further improve the plasticity of the material.
[0085] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, steel billets can be obtained by converter smelting, refining, and continuous casting processes. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for manufacturing a hot-rolled multi-phase 1770MPa grade prestressed stranded wire rod, characterized in that: The manufacturing method thereof comprises: The wire rod is rolled according to the chemical composition of the stranded wire rod, and the chemical composition and mass percentage of the stranded wire rod include: C: 0.69%~0.74%, Si: 0.20%~0.35%, Mn: 0.10%~0.30%, Cr: 0.18%~0.30%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; after the wire rod is spun into a wire rod at a spinning temperature of ≥925°C, it is first subjected to an online molten salt micro-quenching treatment, so that the wire rod is cooled at a cooling rate of ≥39°C / s to enter the bainite phase region, promoting the transformation of part of austenite to bainite, and then subjected to an online molten salt tempering treatment, so that the wire rod is heated to the pearlite phase region for isothermal phase transformation to promote The untransformed austenite is transformed into pearlite, the bainite and pearlite structures are tempered and softened, the carbides are spheroidized, and finally, the wire rod is roller cooled to obtain a wire strand having a microstructure including 71% to 77% tempered pearlite by volume, 17% to 23% tempered bainite by volume, and the rest being a mixed structure composed of tempered ferrite and micro-spheroidized carbides; the molten salt temperature of the online molten salt micro-quenching treatment is 430 to 478°C, and the treatment time is 20 to 40s; the molten salt temperature of the online molten salt tempering treatment is 530 to 570°C, and the treatment time is 300 to 550s; the roller cooling controls the wire rod to slowly cool at a cooling rate of 0.65 to 0.85°C / s until it is coiled.
2. The method for manufacturing the hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to claim 1, characterized in that: Before the rolling, the heating furnace temperature is controlled to be ≤1120°C and the time in the furnace is ≤3h.
3. The method for manufacturing the hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to claim 1, characterized in that: During the rolling, the initial rolling temperature is controlled to be 1060-1100° C., the initial rolling reduction is 25%-35%, the final rolling temperature is ≤955° C., and the final rolling reduction is 28%-38%.
4. The method for manufacturing the hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to claim 1, characterized in that: The molten salt circulation volume of the online molten salt micro-quenching treatment is 450-550 t / h, and the molten salt temperature rise is ≤10°C; the molten salt circulation volume of the online molten salt tempering treatment is 150-350 t / h, and the molten salt temperature rise is ≤5°C.
5. The method for manufacturing the hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to claim 1, characterized in that: After coiling, the wire rod is controlled to be gradually cooled to room temperature at a cooling rate of ≤2°C / s.
6. A hot-rolled multi-phase 1770MPa grade prestressed stranded wire rod, characterized in that: The stranded wire rod is manufactured by the method for manufacturing the hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to any one of claims 1 to 5.
7. The hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to claim 6, characterized in that: The tempered pearlite lamellar spacing of the stranded wire rod is 160-210 nm, the network carbide grade is 0, and the mechanical property circle difference is ≤24 MPa.
8. The hot-rolled multi-phase 1770 MPa grade prestressed stranded wire rod according to claim 6, characterized in that: The wire rod for stranding has a diameter of 8.0-13.0 mm, a tensile strength of 1185-1215 MPa, and a cross-sectional shrinkage of 40%-45%.
Citation Information
Patent Citations
Phi 14 mm high-strength wire rod for manufacturing of 1*(7-21.6) / 1770 MPa prestressed steel strand and production method of phi 10 mm high-strength wire rod
CN104805363A
12.9-grade annealing-free hot-rolled complex-phase cold heading steel wire rod and manufacturing method thereof
CN118166189A
Hot-rolled wire rod for 12.9-grade low-chromium annealing bolt and manufacturing method of hot-rolled wire rod
CN118166190A
10.9-grade non-adjustable cold heading steel hot-rolled wire rod and manufacturing method thereof
CN118166286A
12.9-grade annealing-free hot-rolled high-carbon cold heading steel wire rod and manufacturing method thereof
CN118497622A