CrMoNbV refractory high-entropy alloy and preparation method and application thereof
By laser treatment of CrMoNbV cast alloy under an inert gas atmosphere, a honeycomb BCC double-phase ultrafine crystal microstructure is formed, which solves the problem of both wear resistance and toughness of CrMoNbV alloy, and achieves significant enhancement and toughness of wear resistance The maintenance is suitable for the manufacture of mechanical parts.
Patent Information
- Application Number
- CN202410915207.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-05
AI Technical Summary
The wear resistance of existing CrMoNbV alloys at room temperature and high temperatures is insufficient, making it difficult to meet the needs of long-term service, and existing methods to improve wear resistance often reduce the toughness of the material.
By using laser to treat the surface of the CrMoNbV cast alloy under an inert gas atmosphere, a unique honeycomb BCC biphasic ultrafine crystalline microstructure is formed, which improves the surface hardness and wear resistance of the alloy while maintaining toughness.
The wear resistance of CrMoNbV alloy is significantly improved, the wear rate is reduced, and the toughness of the alloy is not affected, making it have wide application potential in the manufacturing of mechanical parts.
Smart Images

Figure CN118895477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of metal materials, and in particular to a CrMoNbV refractory high entropy alloy and a preparation method and application thereof. Background Art
[0002] In industrial production, friction and wear cause a large amount of material loss every year around the world. For example, in mechanical parts such as bearings, guide rails, and pulleys, wear is one of the important causes of fatigue failure. Improving the wear resistance of metal materials can not only increase the service life of alloy components, but also reduce costs and improve product stability and reliability.
[0003] Refractory high entropy alloys are alloys composed of elements with higher melting points. Compared with traditional alloy materials, refractory high entropy alloys have better mechanical properties at high temperatures. Among them, CrMoNbV refractory high entropy alloys have stable high-temperature mechanical properties and have attracted widespread attention. However, the wear resistance of ordinary CrMoNbV cast alloys is difficult to meet the needs of long-term service, especially at high temperatures. Therefore, improving the room temperature and high temperature wear resistance of CrMoNbV alloys has important engineering value for broadening the application scenarios of this alloy.
[0004] Common methods to improve wear resistance include grain refinement, introduction of nitrides or bulking substances, which can increase the hardness of the material and reduce the wear rate, but such methods reduce the toughness of the material and are difficult to achieve practical application value.
[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a CrMoNbV refractory high entropy alloy and a preparation method and application thereof, aiming to solve the problem that the CrMoNbV alloy prepared by the existing method cannot have both wear resistance and toughness.
[0007] The technical solution of the present invention is as follows:
[0008] A first aspect of the present invention provides a method for preparing a CrMoNbV refractory high entropy alloy, comprising the steps of:
[0009] The metal elements Cr, Mo, Nb and V are mixed and smelted to obtain a CrMoNbV cast alloy;
[0010] In an inert gas atmosphere, the surface of the CrMoNbV cast alloy is treated by laser to obtain a CrMoNbV refractory high entropy alloy, wherein the surface microstructure of the CrMoNbV refractory high entropy alloy is honeycomb-shaped.
[0011] A second aspect of the present invention provides a CrMoNbV refractory high entropy alloy prepared by the method for preparing the CrMoNbV refractory high entropy alloy described in the present invention.
[0012] A third aspect of the present invention provides a use of the CrMoNbV refractory high entropy alloy of the present invention in manufacturing mechanical parts.
[0013] Beneficial effects: The present invention provides a method for improving the wear resistance of CrMoNbV alloy based on surface laser remelting technology. The method is simple and efficient, and the prepared CrMoNbV refractory high entropy alloy has a unique honeycomb BCC dual-phase ultrafine grain microstructure, which improves the surface hardness of the alloy material and achieves a significant increase in wear resistance while maintaining its toughness. Therefore, it is expected to be widely used in the manufacture of mechanical parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is the grain size and grain orientation distribution diagram of the CrMoNbV cast alloy prepared in Comparative Example 1 shown by electron backscatter diffraction (EBSD).
[0015] Figure 2 This is the EDX element distribution diagram of the CrMoNbV cast alloy prepared in Comparative Example 1.
[0016] Figure 3 This is a transmission electron microscope image of the CrMoNbV refractory high entropy alloy prepared in Example 1.
[0017] Figure 4 This is the EDX element distribution diagram of the CrMoNbV refractory high entropy alloy prepared in Example 1.
[0018] Figure 5 This is a comparison chart of friction coefficient curves of the CrMoNbV refractory high entropy alloy prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1.
[0019] Figure 6 This is a comparison diagram of the friction track cross-section of the CrMoNbV refractory high entropy alloy prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1.
[0020] Figure 7 This is a comparison chart of the wear rates of the CrMoNbV refractory high entropy alloy prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1. DETAILED DESCRIPTION
[0021] The present invention provides a CrMoNbV refractory high entropy alloy and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0022] According to one embodiment of the present invention, a method for preparing a CrMoNbV refractory high entropy alloy is provided, characterized in that it comprises the steps of:
[0023] S1. Mix and smelt metal elements Cr, Mo, Nb and V to obtain a CrMoNbV cast alloy;
[0024] S2. In an inert gas atmosphere, using a laser to process the surface of the CrMoNbV cast alloy to obtain a CrMoNbV refractory high entropy alloy, wherein the surface microstructure of the CrMoNbV refractory high entropy alloy is honeycomb-shaped.
[0025] The embodiment of the present invention provides a method for improving the wear resistance of a CrMoNbV alloy based on a surface laser remelting technology. The method comprises the following steps: firstly, a single-phase cast CrMoNbV alloy is prepared by melting a single metal substance, and then the CrMoNbV cast alloy is subjected to surface laser treatment under the assistance of an inert atmosphere. The high temperature generated by the laser causes the alloy surface to be remelted and recrystallized. After the laser treatment, a unique honeycomb BCC dual-phase (dual-phase body-centered cubic structure) ultrafine grain microstructure is formed on the alloy surface due to a high cooling rate, thereby improving the surface hardness of the material and achieving a significant enhancement in wear resistance while maintaining its toughness.
[0026] The advantages of the embodiments of the present invention are that, first, the alloy surface is remelted by laser, and because of the natural rapid cooling, the alloy grains can be refined while the alloy elements are precipitated on the surface to form a unique honeycomb structure and an ultrafine grain microstructure, thereby improving the wear resistance of the alloy; second, the alloy element components can be precipitated by laser remelting to form a BCC dual-phase structure. During the friction process, the two-phase coordinated deformation will form a layered structure on the sub-surface, which can improve the wear resistance of the alloy; third, inert gas is used to assist in laser processing, the alloy material will not oxidize, and the toughness of the alloy will not be greatly reduced, thereby ensuring that the alloy material also has excellent toughness.
[0027] According to one embodiment of the present invention, the purity of the metal elements Cr, Mo, Nb, and V is greater than 99.9%.
[0028] The embodiment of the present invention selects a metal element with a purity greater than 99.9% as a raw material. The higher the purity of the raw material, the less impurities there are, and the better the performance of the CrMoNbV refractory high entropy alloy prepared in this way.
[0029] According to one embodiment of the present invention, the molar ratio of the metal elements Cr, Mo, Nb, and V is 1:1:1:1.
[0030] In the embodiment of the present invention, the CrMoNbV cast alloy is prepared by using metal elements Cr, Mo, Nb, and V in an equal molar ratio. The size of the prepared CrMoNbV cast alloy is 50 μm-200 μm, and it exhibits a single-phase body-centered cubic structure.
[0031] In step S1, in one embodiment, the vacuum degree of the smelting is less than or equal to 1×10 -3 Pa. Within this vacuum range, metal materials are not easily oxidized and have fewer pores.
[0032] In a preferred embodiment, the vacuum degree of the smelting is 1×10 -3 Pa.
[0033] In one embodiment, the smelting is performed in an arc melting furnace.
[0034] In one embodiment, the steps of mixing and smelting the metal elements Cr, Mo, Nb, and V to obtain a CrMoNbV cast alloy specifically include:
[0035] Metal elements Cr, Mo, Nb and V in a molar ratio of 1:1:1:1 are weighed and placed in an arc melting furnace, and the metal elements Cr, Mo, Nb and V are mixed and melted in an argon atmosphere to obtain a CrMoNbV cast alloy.
[0036] In a preferred embodiment, the metal elements Cr, Mo, Nb, and V are mixed and smelted at least three times, so that a more uniformly mixed alloy can be obtained.
[0037] In step S2, in one embodiment, the process parameters of the laser include: laser power of 30W-120W, laser time of 1min-30min, scanning speed of 30mm / s-1000mm / s, and scanning spacing of 50μm-100μm.
[0038] In a preferred embodiment, the laser power is 60 W, the scanning speed is 300 mm / s, and the scanning interval is 50 μm. Under the laser process parameters, the surface microstructure of the prepared CrMoNbV refractory high entropy alloy is uniform and has a large action depth.
[0039] In one embodiment, the scanning method in the laser processing adopts linear single scanning processing or field-shaped repeated scanning processing.
[0040] In one embodiment, the step of using a laser to process the surface of the CrMoNbV cast alloy under an inert gas atmosphere to obtain a CrMoNbV refractory high entropy alloy, wherein the surface microstructure of the CrMoNbV refractory high entropy alloy is honeycomb-shaped specifically comprises:
[0041] In an inert gas atmosphere, a laser is used to process the surface of the CrMoNbV cast alloy, wherein the laser process parameters include: a laser power of 60 W, a scanning speed of 300 mm / s, and a scanning interval of 50 μm, to obtain a CrMoNbV refractory high entropy alloy, wherein the surface microstructure of the CrMoNbV refractory high entropy alloy is honeycomb-shaped.
[0042] In one embodiment, the inert gas is argon or nitrogen.
[0043] According to one embodiment of the present invention, before the step of using laser to process the surface of the CrMoNbV cast alloy, the step further includes: heat treating and polishing the CrMoNbV cast alloy. Heat treating the CrMoNbV cast alloy can effectively eliminate dendrites in the smelted sample and obtain a homogeneous solid solution phase. Polishing the CrMoNbV cast alloy is to unify the initial wear conditions so as to better perform wear resistance tests later.
[0044] In a preferred embodiment, the heat treatment temperature is 1400°C-1800°C, and the heat treatment time is 24h-72h.
[0045] In a preferred embodiment, the heat treatment temperature is 1400° C. and the heat treatment time is 24 hours. At this temperature and time, the dendrites in the smelted sample disappear, so that the CrMoNbV cast alloy obtained by mixed smelting forms a uniform single-phase body-centered cubic structure.
[0046] In a preferred embodiment, the heat treatment is performed in a muffle furnace.
[0047] In a preferred embodiment, the polishing process is to use 1200 mesh sandpaper to polish the CrMoNbV cast alloy.
[0048] According to one embodiment of the present invention, there is provided a CrMoNbV refractory high entropy alloy prepared by the method for preparing the CrMoNbV refractory high entropy alloy of the present invention.
[0049] The CrMoNbV refractory high entropy alloy provided in the embodiment of the present invention has a unique honeycomb BCC dual-phase ultrafine grain microstructure on its surface. During the friction process, the dual-phase coordinated deformation will form a layered structure on the sub-surface, which can improve the wear resistance of the alloy. In addition, due to the refinement of the grains, the surface hardness of the alloy can be increased, thereby improving the wear resistance of the alloy without affecting the toughness inside the alloy.
[0050] According to one embodiment of the present invention, there is provided a use of the CrMoNbV refractory high entropy alloy of the present invention in manufacturing mechanical parts.
[0051] According to one embodiment of the present invention, the mechanical component is one or more of a bearing, a guide rail, a pulley, a hinge and a gear.
[0052] The present invention will be further described below by means of specific examples.
[0053] Example 1
[0054] The CrMoNbV refractory high entropy alloy having a honeycomb BCC dual-phase ultrafine grain microstructure is prepared as follows:
[0055] Step 1: Weigh high-purity (purity greater than 99.9%) metal single substances Cr, Mo, Nb, V blocks, the molar ratio of each metal single substance is 1:1:1:1, put them into an arc melting furnace, and the vacuum degree is 1×10 -3 Pa, using an arc to melt the metal single substance under the protection of argon gas, and remelting at least 3 times to make the alloy elements uniform, to obtain a CrMoNbV cast alloy.
[0056] Step 2, the obtained CrMoNbV cast alloy is placed in a muffle furnace for heat treatment under argon protection, the heat treatment temperature is 1400 ° C, and the time is 24h. The obtained alloy is then cut into 2mm thick sheet samples, and then the alloy is polished with 1200 mesh sandpaper until there are no obvious scratches on the surface. Finally, the surface of the CrMoNbV cast alloy is treated in an argon atmosphere using a large-scale selective laser melting system (Hans-m-100, Hanslaser), where the laser power is 60W, the scanning speed is 300mm / s, the scanning spacing is 50μm, and the scanning is repeated in a field, that is, a CrMoNbV refractory high entropy alloy with a honeycomb BCC dual-phase ultrafine grain microstructure is prepared.
[0057] Comparative Example 1
[0058] Preparation of CrMoNbV cast alloy: A CrMoNbV cast alloy was prepared by the same method as step 1 in Example 1.
[0059] The surface microstructure of the alloys prepared in Example 1 and Comparative Example 1 was tested, and the results were as follows:
[0060] Figure 1 is the grain size and grain orientation distribution diagram of the CrMoNbV cast alloy prepared in Comparative Example 1 shown by electron backscatter diffraction (EBSD), Figure 2 This is the EDX element distribution diagram of the CrMoNbV cast alloy prepared in Comparative Example 1. Figure 1 and Figure 2 It can be seen that the CrMoNbV cast alloy has a single-phase BCC structure and the metal elements are evenly distributed.
[0061] Figure 3 is a transmission electron microscope image of the CrMoNbV refractory high entropy alloy prepared in Example 1, Figure 4 This is the EDX element distribution diagram of the CrMoNbV refractory high entropy alloy prepared in Example 1. Figure 3 and Figure 4 It can be seen that a honeycomb dual-phase BCC structure is formed on the surface of the alloy after laser treatment, and the metal elements have obvious composition differences.
[0062] Experimental method for wear resistance test: Cut the alloy sample into a size of Φ15mm×2mm, and then polish the alloy until there are no obvious scratches on the surface. The alloy sample was subjected to a circular (radius of 3mm) sliding friction and wear test on the Anton Paar THT-800 high temperature friction and wear tester. Ball-disc dry sliding wear was adopted, and the grinding material was a Φ6mm silicon nitride ceramic ball. The wear test was carried out in an atmospheric environment (relative humidity of about 70%) at room temperature (about 25°C), with a friction sliding speed of 0.1m / s, a load of 5N, and a sliding distance of 1000m. After the experiment, the friction coefficient curve was recorded; and the wear track morphology was measured using a 3D profilometer, and the wear rate was calculated based on the wear volume.
[0063] The wear resistance test method was used to test the wear resistance of the CrMoNbV refractory high entropy alloy with a honeycomb BCC dual-phase ultrafine grain microstructure on the surface prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1. The results are as follows:
[0064] Figure 5 is a comparison diagram of the friction coefficient curves of the CrMoNbV refractory high entropy alloy prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1, Figure 6 : is a comparison diagram of the friction track cross-section of the CrMoNbV refractory high entropy alloy prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1. Figure 5-Figure 6It can be seen that compared with the CrMoNbV cast alloy before laser treatment, the CrMoNbV refractory high entropy alloy with a honeycomb BCC dual-phase ultrafine grain microstructure formed by laser treatment in the present invention exhibits better wear resistance.
[0065] Figure 7 : is a comparison chart of the wear rates of the CrMoNbV refractory high entropy alloy prepared in Example 1 and the CrMoNbV cast alloy prepared in Comparative Example 1. According to the figure, the wear rate of the CrMoNbV cast alloy is 6.05×10 -6 mm 3 / Nm, while the wear rate of the CrMoNbV refractory high entropy alloy formed by laser treatment is 3.2×10 -6 mm 3 / Nm, which is significantly reduced by 42%, which also proves that the CrMoNbV refractory high entropy alloy with a honeycomb BCC dual-phase ultrafine grain microstructure formed by laser treatment in the present invention exhibits better wear resistance.
[0066] In summary, the preparation method provided by the present invention is simple and efficient, and the prepared CrMoNbV refractory high entropy alloy has a unique honeycomb BCC two-phase ultrafine grain microstructure, which improves the surface hardness of the alloy material and achieves a significant enhancement in wear resistance while maintaining its toughness.
[0067] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a CrMoNbV refractory high entropy alloy, characterized in that: Includes steps: The metal elements Cr, Mo, Nb and V are mixed and smelted to obtain a CrMoNbV cast alloy; In an inert gas atmosphere, the surface of the CrMoNbV cast alloy is treated by laser to obtain a CrMoNbV refractory high entropy alloy, wherein the surface microstructure of the CrMoNbV refractory high entropy alloy is honeycomb-shaped.
2. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 1, characterized in that: The purity of the metal elements Cr, Mo, Nb and V is greater than 99.9%.
3. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 1, characterized in that: The molar ratio of the metal elements Cr, Mo, Nb and V is 1:1:1:
1.
4. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 1, characterized in that: The vacuum degree of the smelting is less than or equal to 1×10 -3 Pa.
5. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 1, characterized in that: The process parameters of the laser include: laser power of 30W-120W, laser time of 1min-30min, scanning speed of 30mm / s-1000mm / s, and scanning spacing of 50μm-100μm.
6. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 1, characterized in that: Before the step of using laser to process the surface of the CrMoNbV cast alloy, the method further comprises the steps of: subjecting the CrMoNbV cast alloy to heat treatment and polishing.
7. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 6, characterized in that: The temperature of the heat treatment is 1400° C.-1800° C., and the time of the heat treatment is 24 h-72 h.
8. The method for preparing the CrMoNbV refractory high entropy alloy according to claim 1, characterized in that: The inert gas is argon or nitrogen.
9. A CrMoNbV refractory high entropy alloy prepared by the method for preparing a CrMoNbV refractory high entropy alloy as described in any one of claims 1 to 8.