ZrCu modified CVD-SiC anti-ablation coating and preparation method thereof
A dense ZrCu-modified CVD-SiC coating was prepared by depositing a SiC coating on the surface of C/C composite material and utilizing the molten salt reaction of ZrCu powder. This solved the problems of complex process and poor protective effect in the prior art, and achieved effective protection of C/C composite material at high temperature.
Patent Information
- Application Number
- CN202411202637.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing technology for preparing ablation-resistant coatings for C/C composite materials is complex and has limited protective effect in high-temperature environments. The coating is prone to damaging the substrate, has poor adhesion, and high porosity, making it difficult to provide effective protection in high-temperature oxidizing environments.
After depositing a SiC coating on the surface of a C/C composite material using chemical vapor deposition, a dense ZrCu-modified CVD-SiC ablation-resistant coating is formed by molten salt reaction of mixed ZrCu powder, ZrO2 powder, and NaCl-NaF powder, followed by heat treatment in an inert atmosphere. The coating consists of an inner SiC layer and a Zr-Cu-Si layer and is prepared at a relatively low temperature through simple process operations.
The prepared ZrCu modified CVD-SiC coating exhibits good ablation resistance under high-temperature ablation environment. The surface temperature decreases, the mass and linear ablation rate decrease, the coating has high density and uniform composition distribution, providing effective substrate protection and avoiding coating peeling and damage.
Smart Images

Figure CN118895488A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ablation protection coatings, and specifically relates to a ZrCu modified CVD-SiC ablation-resistant coating and a preparation method thereof. Background Art
[0002] Carbon / carbon (C / C) composites have the advantages of low density, low thermal expansion coefficient, high specific strength, high specific modulus, high thermal conductivity, good thermal shock resistance and ablation resistance. At the same time, as the only material whose strength increases with temperature between 1000℃ and 2400℃, it has become one of the most promising materials in the field of thermal protection. However, C / C composites are very easy to oxidize in high-temperature (above 400℃) oxygen environment, and show high oxidation sensitivity with the increase of temperature, which causes the carbon fiber, matrix and the interface between fiber and matrix to be severely damaged when serving in high-temperature environment, and its mechanical properties are seriously reduced, thus causing the failure of C / C composites. Silicon-based ceramic coating technology is an important technology that can achieve long-term and effective protection of C / C composites. Among them, SiC coatings prepared by chemical vapor deposition technology are ideal for ablation protection coating materials because of their high thermal expansion adaptability to C / C composites and relatively low preparation temperature, which has little damage to the mechanical properties of the material and generates glassy SiO2 with self-healing properties at high temperature.
[0003] However, in an ablation environment above 1700°C, the viscosity of glassy SiO2 is low and its fluidity is high, so it is easily blown away from the surface of the C / C composite material by high-temperature airflow. Above 2000°C, SiO2 will volatilize rapidly, causing damage to the coating and failing to provide effective protection for the C / C matrix. Studies have shown that the introduction of ultra-high temperature refractory metal elements such as Zr into SiC coatings can stabilize SiO2, prevent glassy SiO2 from being washed away by airflow, avoid cracking of the coating, increase the density of SiC coatings at higher ablation temperatures, and improve the protective effect of the coating. In Paper 1, "GHFeng, HJLi, XYYao, B.Ren, YJJia, J.Sun et al. Evaluation of ablation resistant ZrC-SiC multilayer coating for SiC coated carbon / carbon composites under oxyacetylene and laser condition[J]. CorrosionScince, 2022, 205: 110427.", a SiC transition layer was first prepared on the surface of the C / C composite material by the embedding method, and then ZrC-SiC coatings with different ZrC / SiC ratios were prepared on the SiC coating by atmospheric plasma spraying technology. The inner layer SiC was used to alleviate the thermal mismatch of the coating. The glassy Zr-Si-O formed by the high-temperature oxidation of ZrC-SiC closed the pores of the coating during the short-time ablation process at a temperature of up to 2000°C to form a dense oxide layer. However, this process requires embedding, granulation, spraying and other processes to prepare the coating, which is cumbersome. The preparation temperature of the SiC inner coating is high (2100°C), which will cause great damage to the C / C substrate. In addition, there is a large porosity in the coating prepared by plasma spraying, and the protective effect of the coating is limited. Paper 2 "B. Li, HJ Li, XY Yao et al. Ablation behavior of the CVD-(ZrC / SiC)3 alternate coating on C / C composites under oxyacetylene torch with different heat fluxes [J]. Ceramics International, 2022, 48: 11756-11763." The (ZrC / SiC)3 alternating coating was prepared on the surface of C / C composite by CVD process. SiC was introduced between the C / C composite matrix and ZrC and between adjacent ZrC coatings to alleviate the thermal mismatch of the coating. During the ablation process, the high melting point ZrO2 stabilized the glassy SiO2, but the ablation temperature was too high (>2100℃). After the SiO2 in the alternating coating volatilized, gaps would be formed, resulting in the destruction of the structural integrity of the coating.In addition, the process is cumbersome, and the bonding between the coating and the substrate and between the coatings is poor, resulting in poor thermal shock resistance of the coating. Patent 1 "Chen Zhaoke, Xiong Xiang, Wang Xinshuang, Sun Wei, Wang Yalei, Huang Jie. Preparation method of ZrC-SiC coating on C / C composite surface, CN201510653315.0[P].2017" adopts a slurry brushing / dipping-high temperature sintering method. First, a Zr-Si-permeation agent-slag forming agent ceramic slurry is prepared, and then it is brushed on the C / C surface. After sintering, a ZrC-SiC coating is obtained. However, the preparation process is relatively complicated, the coating thickness uniformity is poor after slurry brushing, the reaction temperature is high, the damage to the C / C substrate is large, and the coating porosity is high. Therefore, in order to achieve effective protection of C / C composites in high-temperature ablation environments, it is necessary to prepare a multiphase anti-ablation coating with good coating bonding effect, excellent self-healing performance, low preparation temperature, less damage to the substrate, simple and controllable process, and the ability to reduce the surface temperature during ablation. Summary of the invention
[0004] The object of the present invention is to provide a ZrCu modified CVD-SiC anti-ablation coating and a preparation method thereof, so as to solve the technical problem of complex preparation process in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The invention discloses a method for preparing a ZrCu modified CVD-SiC anti-ablation coating, comprising the following steps:
[0007] On the surface of the C / C composite material, a SiC coating is deposited by chemical vapor deposition using methyltrichlorosilane as a raw material to obtain a C / C composite material having a SiC coating on the surface;
[0008] The ZrCu powder, ZrO2 powder and NaCl-NaF powder are mixed to obtain a mixed powder; a C / C composite material having a SiC coating on the surface is buried in the mixed powder, and then heat-treated in an inert atmosphere; and then washed and dried in sequence to obtain a ZrCu modified CVD-SiC anti-ablation coating on the surface of the C / C composite material.
[0009] Furthermore, the chemical vapor deposition uses H2 as a reaction gas and Ar as a dilution gas and is performed in a negative pressure environment.
[0010] Furthermore, the Ar flow rate is 100-400 mL / min, the H2 flow rate is 800-1500 mL / min, and the pressure of the negative pressure environment is 4-6 kPa; the temperature during the chemical vapor deposition is 1100-1300° C., and the flow rate of methyltrichlorosilane is 0.2-0.4 g / min.
[0011] Furthermore, the molar ratio of the ZrCu powder to the NaCl-NaF powder is (1:2) to (1:6); the molar ratio of the ZrCu powder to the ZrO2 powder is (10:1) to (1:3).
[0012] Furthermore, the NaCl-NaF powder is obtained by mixing NaCl powder and NaF powder in a molar ratio of (6:1) to (2:1).
[0013] Furthermore, the purity of the ZrCu powder is 99.9%, and the particle size is 200 mesh; the purity of the ZrO2 powder is 99.5%, and the particle size is 1-3 μm; the purity of the NaCl powder and the NaF powder are both 99.5%.
[0014] Furthermore, the heat treatment is performed at a temperature of 1300 to 1500° C. and for a time of 1 to 4 hours.
[0015] Furthermore, the inert atmosphere is an Ar atmosphere at normal pressure.
[0016] Furthermore, the cleaning is performed by ultrasonic cleaning with deionized water at 70 to 80°C for 12 to 48 hours; and the temperature of the drying treatment is 70 to 80°C.
[0017] The invention also discloses a ZrCu modified CVD-SiC ablation-resistant coating prepared by the preparation method.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention discloses a method for preparing a ZrCu modified CVD-SiC anti-ablation coating. A C / C composite material with a SiC coating on its surface is buried in a mixed powder consisting of ZrCu powder, ZrO2 powder and NaCl-NaF powder, and Zr and Cu elements are introduced into the SiC coating through a molten salt reaction, forming a Zr-Si-Cu mosaic structure inside the coating to form a ZrCu modified CVD-SiC anti-ablation coating with high density and relatively uniform component distribution. The method can prepare a ZrCu modified CVD-SiC anti-ablation coating with high density and relatively uniform component distribution at a relatively low temperature (1300-1500°C) through simple process operation and heat treatment equipment, without repeated deposition or multiple complex high-temperature reactions, and the preparation process is simple and easy to control.
[0020] The present invention also discloses a ZrCu modified CVD-SiC anti-ablation coating prepared by the above preparation method. The prepared coating consists of an internal SiC layer and a Zr-Cu-Si layer composed of Si-rich SiC, C-rich SiC, and Zr-containing phases and Cu-containing phases uniformly embedded therein. The thickness of the Zr-Cu-Si layer can be adjusted by controlling the reaction time and the reaction temperature, and the density of the coating is not reduced. According to relevant experimental results, the coating has a flow rate of 2.38MW / m 2 After 60s of ablation under an oxyacetylene flame, the mass ablation rate and line ablation rate are -0.44mg / s and -0.24μm / s, respectively, and the surface temperature is about 1980℃, which is about 200℃ lower than that of conventional Zr-containing coatings during ablation (2160℃). The coating shows a thickening phenomenon, and the surface SiO2 does not undergo obvious stripping under the stabilizing effect of ZrO2 and the cooling effect of Cu. At the same time, the surface ZrO2 is well sintered, which can provide effective protection for the substrate, and the coating shows good anti-ablation performance. Under the same ablation conditions, the unmodified CVD-SiC coating shows intercrystalline loss behavior during the ablation process, and the surface SiO2 is consumed in large quantities through airflow scouring and volatilization. The mass ablation rate and line ablation rate reach 0.06mg / s and 0.05μm / s, respectively. The above phenomena indicate that compared with the SiC coating, the ablation performance of the ZrCu-modified coating is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The XRD spectrum of the ZrCu modified CVD-SiC anti-ablation coating prepared by the present invention;
[0022] Figure 2 The SEM images of the surface and cross section of the ZrCu modified CVD-SiC anti-ablation coating prepared by the present invention;
[0023] Where: a-surface; b-section;
[0024] Figure 3 The unmodified CVD-SiC coating and the ZrCu modified CVD-SiC ablation-resistant coating of the present invention are 2.38M / Wm 2 Surface temperature curves and mass and linear ablation rate diagrams of 60s ablation under oxyacetylene heat flux;
[0025] Wherein: a-surface temperature curve; b-mass and line ablation rate diagram;
[0026] Figure 4 The surface macroscopic morphology of the unmodified CVD-SiC coating and the ZrCu modified CVD-SiC ablation-resistant coating of the present invention before and after ablation;
[0027] Where: a-before ablation; b-after ablation;
[0028] Figure 5 The surface SEM images of the unmodified CVD-SiC coating and the ZrCu modified CVD-SiC ablation-resistant coating of the present invention before and after ablation;
[0029] Among them: a-unmodified CVD-SiC coating; b-ZrCu modified CVD-SiC coating. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0031] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0032] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions).
[0033] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0034] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0035] A first aspect of the present invention provides a method for preparing a ZrCu modified CVD-SiC anti-ablation coating, comprising the following steps:
[0036] Step 1: placing the polished, cleaned and dried C / C composite material in a constant temperature zone of a vertical chemical vapor deposition furnace, using H2 as a reaction gas, Ar as a dilution gas, and methyltrichlorosilane (MTS) as a raw material, and depositing a SiC coating by chemical vapor deposition under a negative pressure environment to obtain a C / C composite material with a SiC coating on the surface;
[0037] Step 2: Mix ZrCu powder, ZrO2 powder and NaCl-NaF powder to obtain mixed powder; bury the C / C composite material with SiC coating on the surface into the mixed powder and place it in a crucible, and finally seal the crucible;
[0038] Step 3: placing the sealed crucible in the constant temperature zone of a tube furnace, and then performing heat treatment in an inert atmosphere at normal pressure; then performing cleaning and drying treatments in sequence to obtain a ZrCu modified CVD-SiC anti-ablation coating on the surface of the C / C composite material.
[0039] Preferably, the Ar flow rate is 100-400 mL / min, the H2 flow rate is 800-1500 mL / min, and the pressure of the negative pressure environment is 4-6 kPa; the temperature during the chemical vapor deposition is 1100-1300° C., and the flow rate of methyltrichlorosilane is 0.2-0.4 g / min.
[0040] Preferably, the molar ratio of the ZrCu powder to the NaCl-NaF powder is (1:2) to (1:6); the molar ratio of the ZrCu powder to the ZrO2 powder is (10:1) to (1:3).
[0041] Preferably, the NaCl-NaF powder is obtained by mixing NaCl powder and NaF powder in a molar ratio of (6:1) to (2:1).
[0042] Preferably, the purity of the ZrCu powder is 99.9% and the particle size is 200 mesh; the purity of the ZrO2 powder is 99.5% and the particle size is 1-3 μm; the purity of the NaCl powder and the NaF powder are both 99.5%.
[0043] Preferably, the heat treatment is performed at a temperature of 1300 to 1500° C. and for a time of 1 to 4 hours.
[0044] Preferably, the cleaning is performed by ultrasonic cleaning with deionized water at 70-80°C for 12-48 hours; and the temperature of the drying treatment is 70-80°C.
[0045] The second aspect of the present invention discloses a ZrCu modified CVD-SiC anti-ablation coating prepared by the above preparation method.
[0046] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0047] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0048] Example 1
[0049] A method for preparing a ZrCu modified CVD-SiC anti-ablation coating comprises the following steps:
[0050] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then vacuumed to 4kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1150°C at a heating rate of 5°C / min in an Ar atmosphere. During the heating period, the Ar flow rate is 200mL / min. After reaching the temperature, H2 and MTS with flow rates of 1000mL / min and 0.3g / min are introduced, respectively, to deposit a SiC coating on the surface of the C / C composite material. After the deposition is completed, H2 and MTS are turned off, the power is turned off, the Ar flow rate is maintained at 200mL / min and the temperature is lowered with the furnace. After it drops to room temperature, a C / C composite material with a SiC coating on the surface is obtained;
[0051] Weigh 2.7 g of ZrCu powder with a particle size of 200 mesh, 5.9 g of NaCl powder with a particle size of 1 to 10 μm, 2.7 g of NaF powder, and 1.7 g of ZrO2 powder, and grind the four powders in an agate mortar for 30 minutes to obtain a mixed powder; then bury the C / C composite material with SiC coating on the surface into the mixed powder in an alumina crucible, and then seal the crucible, place the sealed crucible in a constant temperature zone of a horizontal tube furnace, and heat treat it in an Ar environment at 1300°C for 3 hours. After the insulation is completed, turn off the heating power, and cool the sample along with the furnace. The heat-treated sample is ultrasonically cleaned for multiple times in deionized water at 80°C for 12 hours, and then placed in a 70°C oven for drying for 2 hours to obtain a ZrCu modified CVD-SiC anti-ablation coating.
[0052] The Zr—Cu—Si layer of the ZrCu modified CVD-SiC anti-ablation coating in this embodiment is about 45 μm.
[0053] Example 2
[0054] A method for preparing a ZrCu modified CVD-SiC anti-ablation coating comprises the following steps:
[0055] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then vacuumed to 4kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1250°C at a heating rate of 5°C / min in an Ar atmosphere. During the heating period, the Ar flow rate is 200mL / min. After reaching the temperature, H2 and MTS with flow rates of 1200mL / min and 0.4g / min are introduced, respectively, to deposit a SiC coating on the surface of the C / C composite material. After the deposition is completed, H2 and MTS are turned off, the power is turned off, the Ar flow rate is maintained at 200mL / min and the temperature is lowered with the furnace. After it drops to room temperature, a C / C composite material with a SiC coating on the surface is obtained;
[0056] Weigh 4.3 g of ZrCu powder with a particle size of 200 mesh, 8.5 g of NaCl powder with a particle size of 1 to 10 μm, 3.9 g of NaF powder, and 2.1 g of ZrO2 powder, and grind the four powders in an agate mortar for 30 minutes to obtain a mixed powder; then bury the C / C composite material with SiC coating on the surface into the mixed powder in an alumina crucible, and then seal the crucible, place the sealed crucible in a constant temperature zone of a horizontal tube furnace, and heat treat it in an Ar environment at 1400°C for 4 hours. After the insulation is completed, turn off the heating power, and cool the sample with the furnace. The heat-treated sample is ultrasonically cleaned multiple times in deionized water at 80°C for 48 hours, and then placed in a 70°C oven for drying for 2 hours to obtain a ZrCu modified CVD-SiC anti-ablation coating.
[0057] The Zr—Cu—Si layer of the ZrCu modified CVD-SiC anti-ablation coating in this embodiment is about 120 μm.
[0058] Example 3
[0059] A method for preparing a ZrCu modified CVD-SiC anti-ablation coating comprises the following steps:
[0060] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then vacuumed to 4kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1200°C at a heating rate of 5°C / min in an Ar atmosphere. During the heating period, the Ar flow rate is 150mL / min. After reaching the temperature, H2 and MTS with flow rates of 900mL / min and 0.2g / min respectively are introduced to deposit SiC coating on the surface of the C / C composite material. After the deposition is completed, H2 and MTS are turned off, the power is turned off, the Ar flow rate is maintained at 200mL / min and the temperature is lowered with the furnace. After it drops to room temperature, a C / C composite material with SiC coating on the surface is obtained;
[0061] Weigh 6.5 g of ZrCu powder with a particle size of 200 mesh, 13.8 g of NaCl powder with a particle size of 1 to 10 μm, 6.1 g of NaF powder, and 3.8 g of ZrO2 powder, and grind the four powders in an agate mortar for 30 minutes to obtain a mixed powder; then bury the C / C composite material with SiC coating on the surface into the mixed powder in an alumina crucible, and then seal the crucible, place the sealed crucible in a constant temperature zone of a horizontal tube furnace, and heat treat it in an Ar environment at 1500°C for 4 hours. After the insulation is completed, turn off the heating power, and cool the sample with the furnace. The heat-treated sample is ultrasonically cleaned for multiple times in deionized water at 80°C for 12 hours, and then placed in a 70°C oven for 2 hours to obtain a ZrCu modified CVD-SiC anti-ablation coating.
[0062] The Zr—Cu—Si layer of the ZrCu modified CVD-SiC anti-ablation coating in this embodiment has a thickness of about 155 μm.
[0063] Example 4
[0064] A method for preparing a ZrCu modified CVD-SiC anti-ablation coating comprises the following steps:
[0065] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then evacuated to 4 kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1200°C at a heating rate of 5°C / min in an Ar atmosphere. During the heating period, the Ar flow rate is 100 mL / min. After reaching the temperature, H2 and MTS are introduced with flow rates of 800 mL / min and 0.4 g / min, respectively, to deposit a SiC coating on the surface of the C / C composite material. After the deposition is completed, H2 and MTS are turned off, the power is turned off, the Ar flow rate is maintained at 100 mL / min and the temperature is lowered with the furnace. After it drops to room temperature, a C / C composite material with a SiC coating on the surface is obtained;
[0066] Weigh 6.5 g of ZrCu powder with a particle size of 200 mesh, 13.8 g of NaCl powder with a particle size of 1 to 10 μm, 6.1 g of NaF powder, and 3.8 g of ZrO2 powder, and grind the four powders in an agate mortar for 30 minutes to obtain a mixed powder; then bury the C / C composite material with SiC coating on the surface into the mixed powder in an alumina crucible, and then seal the crucible, place the sealed crucible in a constant temperature zone of a horizontal tube furnace, and heat treat it in an Ar environment at 1300°C for 1 hour. After the insulation is completed, turn off the heating power, and cool the sample along with the furnace. The heat-treated sample is ultrasonically cleaned multiple times in deionized water at 80°C for 48 hours, and then placed in a 70°C oven for 2 hours to obtain a ZrCu modified CVD-SiC anti-ablation coating.
[0067] Comparative Example 1
[0068] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then evacuated to 4kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1150°C at a heating rate of 5°C / min in an Ar atmosphere, and the Ar flow rate during the heating period is 200mL / min; after reaching the temperature, H2 and MTS are introduced with flow rates of 1200mL / min and 0.35g / min respectively. After the deposition is completed, H2 and MTS are turned off, the power is turned off, and the Ar flow rate is maintained at 200mL / min and cooled with the furnace. After it drops to room temperature, a C / C composite material containing a SiC coating can be obtained;
[0069] Weigh about 6.7g of ZrCu powder with a particle size of 200 mesh, weigh about 2.9g of NaCl with a particle size of 1-10μm, and about 3.7g of NaF, and grind the three powders in an agate mortar for 30 minutes. Then, bury the C / C composite material containing SiC coating in the mixed powder in an alumina crucible, and then seal the crucible; place the sealed crucible in the constant temperature zone of a horizontal tube furnace and heat treat it in an Ar environment of 1400℃ for 2h; after the insulation is completed, turn off the heating power supply, and cool the sample with the furnace. The heat-treated sample is ultrasonically cleaned several times in deionized water at 80℃, and then placed in a 70℃ oven for 2h. Due to the severe sintering of ZrCu, the sample is adhered to the crucible and cannot be effectively removed, and the surface of the sample is severely damaged.
[0070] Comparative Example 2
[0071] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then evacuated to 4kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1150°C at a heating rate of 5°C / min in an Ar atmosphere, and the Ar flow rate during the heating period is 200mL / min; after reaching the temperature, H2 and MTS are introduced with flow rates of 900mL / min and 0.3g / min respectively. After the deposition is completed, H2 and MTS are turned off, the power is turned off, and the Ar flow rate is maintained at 200mL / min and cooled with the furnace. After it drops to room temperature, a C / C composite material containing a SiC coating can be obtained;
[0072] Weigh about 4.3g of ZrCu powder with a particle size of 200 mesh, weigh about 7.8g of NaCl with a particle size of 1-10μm, about 3.9g of NaF, and about 2.5g of ZrO2 powder, and grind the four powders in an agate mortar for 30 minutes; then bury the above-mentioned C / C composite material containing SiC coating in the mixed powder in an alumina crucible, and then seal the crucible; place the sealed crucible in the constant temperature zone of a horizontal tube furnace and heat treat it in an Ar environment of 1600℃ for 2h; after the insulation is completed, turn off the heating power supply and cool the sample with the furnace; the heat-treated sample is ultrasonically cleaned several times in deionized water at 80℃, and then dried in an oven at 70℃ for 2h, and the surface coating of the obtained sample is obviously cracked and peeled off over a large area, and the coating is seriously damaged.
[0073] Comparative Example 3
[0074] The polished, cleaned and dried C / C composite material is placed in the constant temperature zone of the chemical vapor deposition furnace, and then evacuated to 4kPa, and the air tightness of the equipment is tested by pressure maintenance. If the air tightness is good, the temperature of the constant temperature zone is raised to 1250°C at a heating rate of 5°C / min in an Ar atmosphere, and the Ar flow rate during the heating period is 200mL / min; after reaching the temperature, H2 and MTS are introduced with flow rates of 1200mL / min and 0.4g / min respectively. After the deposition is completed, H2 and MTS are turned off, the power is turned off, and the Ar flow rate is maintained at 200mL / min and cooled with the furnace. After it drops to room temperature, a C / C composite material containing a SiC coating can be obtained;
[0075] Weigh about 6.3g of ZrCu powder with a particle size of 200 mesh, weigh about 14.5g of Na2SO4 with a particle size of 1-10μm, about 4.9g of K2SO4, and about 3.1g of ZrO2 powder, and grind the four powders in an agate mortar for 30 minutes; then bury the above-mentioned C / C composite material containing SiC coating in the mixed powder in an alumina crucible, and then seal the crucible. Place the sealed crucible in the constant temperature zone of a horizontal tube furnace and heat treat it in an Ar environment at 1500℃ for 4h; after the insulation is completed, turn off the heating power supply and cool the sample with the furnace. The heat-treated sample is ultrasonically cleaned several times in deionized water at 80℃, and then placed in a 70℃ oven for 2h. The obtained sample coating is severely corroded, and the surface coating peels off over a large area.
[0076] Figure 1 This is the XRD spectrum of the surface of the ZrCu modified CVD-SiC anti-ablation coating prepared by this method. It can be seen from the figure that through the molten salt reaction, ZrCu reacts with the SiC coating prepared by the CVD method to generate compounds such as Zr3Cu4Si6 and Cu4Si, and together with SiC and ZrC form a Zr-Cu-Si composite coating.
[0077] Figure 2 The surface of the ZrCu modified CVD-SiC anti-ablation coating prepared by this method ( Figure 2 a) and cross section ( Figure 2 b) SEM image. It can be seen from the figure that the surface of the ZrCu modified CVD-SiC anti-ablation coating is dense. The cross-section shows that the coating is composed of an inner SiC layer and an outer Zr-Cu-Si composite coating. Zr3Cu4Si6 and Cu4Si are tightly embedded in the Zr-Cu-Si layer. The coatings and the coatings and the substrate are tightly bonded.
[0078] Figure 3 The surface temperature curve of ZrCu modified CVD-SiC coating in oxyacetylene flame ablation test ( Figure 3 a) and the mass ablation rate and line ablation rate of the coating after ablation ( Figure 3 b), it can be seen from the figure that compared with the unmodified CVD-SiC coating, the maximum ablation temperature of the SiC coating surface after ZrCu modification is significantly reduced, the mass and linear ablation rate of the coating are reduced, and the ablation performance of the coating is enhanced.
[0079] Figure 4 For unmodified CVD-SiC coating ( Figure 4 a) and ZrCu modified CVD-SiC coating ( Figure 4b) Actual pictures before and after ablation. It can be seen from the figure that after ablation, the surface oxide layer of the unmodified CVD-SiC coating falls off in a large area, and the C / C matrix is exposed in the ablation center. However, the surface oxide layer of the ZrCu modified CVD-SiC coating only peels off slightly after ablation, and the oxide layer remains relatively intact.
[0080] Figure 5 For unmodified CVD-SiC coating ( Figure 5 a) and ZrCu modified CVD-SiC coating ( Figure 5 b) SEM image of the surface oxide layer after ablation. It can be seen from the figure that the glassy SiO2 of the unmodified CVD-SiC coating has high fluidity during ablation and is peeled off the sample surface after volatilization and airflow impact. After ZrCu modification, the Zr-Si-O particles in the Zr-Cu-Si composite coating pin the glassy SiO2, and the low melting point phases such as Cu in the coating volatilize to reduce the ablation surface temperature, effectively reduce the loss of the SiC coating, stabilize the surface oxide film, and improve the ablation performance of the SiC coating.
[0081] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a ZrCu modified CVD-SiC anti-ablation coating, It is characterized in that The following steps are involved: On the surface of the C / C composite material, a SiC coating is deposited by chemical vapor deposition using methyltrichlorosilane as a raw material to obtain a C / C composite material having a SiC coating on the surface; ZrCu powder, ZrO 2 The powder and the NaCl-NaF powder are mixed to obtain a mixed powder; a C / C composite material having a SiC coating on the surface is buried in the mixed powder, and then heat-treated in an inert atmosphere; and then cleaning and drying are performed in sequence to obtain a ZrCu modified CVD-SiC anti-ablation coating on the surface of the C / C composite material.
2. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 1, It is characterized in that The chemical vapor deposition is based on H 2 The reaction gas is Ar and the diluent gas is Ar. The reaction is carried out under negative pressure.
3. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 2, It is characterized in that The Ar flow rate is 100-400 mL / min, and the H 2 The flow rate is 800-1500 mL / min, and the pressure of the negative pressure environment is 4-6 kPa; the temperature during the chemical vapor deposition is 1100-1300° C., and the flow rate of methyltrichlorosilane is 0.2-0.4 g / min.
4. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 1, It is characterized in that The molar ratio of the ZrCu powder to the NaCl-NaF powder is (1:2) to (1:6); the ZrCu powder and ZrO 2 The molar ratio of the powder is (10:1) to (1:3).
5. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 1, It is characterized in that The NaCl-NaF powder is obtained by mixing NaCl powder and NaF powder in a molar ratio of (6:1) to (2:1).
6. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 5, It is characterized in that The ZrCu powder has a purity of 99.9% and a particle size of 200 meshes; 2 The powder has a purity of 99.5% and a particle size of 1 to 3 μm; the purity of the NaCl powder and the NaF powder are both 99.5%.
7. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 1, It is characterized in that The heat treatment temperature is 1300-1500° C. and the time is 1-4 hours.
8. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 1, It is characterized in that The inert atmosphere is an Ar atmosphere at normal pressure.
9. The method for preparing a ZrCu modified CVD-SiC anti-ablation coating according to claim 1, It is characterized in that The cleaning is performed by ultrasonic cleaning with deionized water at 70 to 80°C for 12 to 48 hours; the temperature of the drying treatment is 70 to 80°C.
10. A ZrCu modified CVD-SiC anti-ablation coating, It is characterized in that The preparation method is described in any one of claims 1 to 9.
Citation Information
Patent Citations
C / ZrC-SiC-Cu composite material and preparation method thereof
CN103469122A
High-temperature-resistant anti-ablation modified ZrC-SiC ceramic coating and preparation method
CN108129167A
Preparation method of integrated anti-ablation ZrC / SiC-C / C composite
CN108147842A
Matrix-coating layer modified carbon / carbon composite material and preparation process thereof
CN108892542A
C / C-SiC-Cu composite material and preparation method thereof
CN112573937A