Preparation method of composite insulating film layer of heat flow sensor for bearing
By combining the sol gel solution and the CVD-Al2O3 film layer, a composite insulating film structure is formed, which solves the problem of attenuation of conductivity and insufficient thickness of the alumina insulating layer at high temperatures, and achieves the improvement of high-temperature electrical insulation in a high temperature environment and enhanced membrane stability, suitable for bearing heat flow sensors.
Patent Information
- Application Number
- CN202410909662.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-05
AI Technical Summary
The existing magnetron sputtering alumina insulating layer prepared by insulating alumina at high temperatures has problems such as attenuation of conductivity, volume shrinkage, and insufficient adhesion and thickness, making it difficult to provide sufficient electrical insulation in a high temperature environment, affecting the heat flow sensor performance of the bearing.
The sol gel solution and the CVD-Al2O3 film layer are combined, and the barrier layer and the insulating layer are prepared by spin coating to form a composite insulating film structure, increasing the film layer thickness and reducing the diffusion of atoms such as Ti, and improving high-temperature electrical insulation.
It achieves the improvement of the thickness and stability of the insulating layer under high temperature environments, reduces the diffusion of Ti atoms, broadens the use temperature range of the film layer, and is suitable for working environments of 950℃-1000℃.
Smart Images

Figure CN118895489A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of insulating films for thermal flow sensors of bearings, and in particular to a method for preparing a composite insulating film layer for thermal flow sensors of bearings. Background Art
[0002] Bearings play an important role in the aerospace industry, such as aircraft engines and spacecraft propulsion systems. The performance and reliability of bearings directly affect the safety and life of aerospace equipment. Therefore, aerospace bearings need to undergo rigorous design, manufacturing, and testing. In these applications, the operating temperature of bearings has reached over 1000°C, far exceeding the melting point of bearing materials such as nickel-based alloys. In order to protect the bearings from being ablated by high-temperature airflow, high-temperature bearings need to be made into cooling channels to reduce the surface temperature and ensure that the bearings can operate normally when the hot airflow passes through. The indicator for evaluating the rationality of the cooling structure is the heat flux density. The heat flux density refers to the amount of heat passing through the bearing per unit time. By making a thin film heat flux sensor (HFS) on the surface of a high-temperature bearing, the heat flux density of the high-temperature bearing can be obtained, so as to further understand the heat conduction of the bearing in a high-temperature environment, and then optimize the design of the high-temperature bearing and improve the performance and life of the high-temperature bearing.
[0003] The preparation and performance of thin-film thermal flow sensors on the surface of nickel-based alloys are studied, among which the high-temperature insulation of the insulating layer is one of the key factors. There are three problems in the conventional magnetron sputtering preparation of aluminum oxide insulating layers: 1) In the magnetron sputtering process, the maximum preparation temperature of the aluminum oxide insulating layer cannot exceed 600°C. In order to convert the aluminum oxide crystal form into an α-phase structure, a long-term heat treatment of more than 1000°C is required. During this period, the main metal elements of the transition layer and the substrate diffuse into the aluminum oxide insulating layer to form NiFe compounds and Cr2O3. These substances have a certain conductivity at high temperatures, resulting in a sharp attenuation of the high-temperature electrical insulation of the aluminum oxide film; 2) The volume shrinkage of the aluminum oxide crystal form during the phase change destroys the adhesion of the film layer on the alloy surface; 3) Due to the limitation of the magnetron sputtering equipment, the aluminum oxide deposition thickness is too thin (1μm), which cannot provide sufficient electrical insulation under high temperature conditions. The use of high-temperature gas phase product can increase the thickness of the aluminum oxide film and improve the electrical insulation of the film structure under high temperature environment. However, bearings need to serve for a long time in high-temperature environments. Metal atoms in transition layers such as Ti and Cr and on the surface of alloys will still appear in large numbers on the surface of the film layer through diffusion, and react with O2 to form high-temperature conductive oxides. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a composite insulating film layer for a heat flow sensor for a bearing, wherein a barrier layer and a CVD-Al2O3 film layer are prepared using a sol-gel solution to form a composite insulating film structure; the preparation of the composite film layer not only increases the thickness of the insulating film, but also introduces an interface barrier to reduce the diffusion of atoms such as Ti.
[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is: a method for preparing a composite insulating film layer for a heat flow sensor of a bearing, comprising the following steps:
[0006] Step 1: After mechanical grinding, GH3536 nickel-based high-temperature hard alloy is placed in a chemical reaction furnace;
[0007] Step 2: First, CH3CN (acetonitrile), TiCl4, etc. are used as the main reaction raw material gases to generate TiN and Ti(C,N) composite film layers at about 900°C as the transition layer of the nickel-based substrate thin film heat flow sensor. The chemical reaction equation is:
[0008] TiCl4+CH3CN+H2+N2→Ti(C, N)+CH4+HCl
[0009] Step 3: AlCl3, H2 and CO2 are introduced to react at 1000°C to generate α-Al2O3 as an insulating layer. The chemical reaction equation is:
[0010] 2AlCl3+3H2+3CO2→Al2O3+3CO+6HCl Step 4: Spin-coat the surface of the Al2O3 film layer with the A-4-10 acidic aluminum sol-gel solution to prepare a Sol-gel-Al2O3 barrier layer;
[0011] Step 5: annealing the composite film layer obtained in step 4 to obtain a composite insulating film layer.
[0012] Preferably, in step five, the annealing heating rate is 2°C / min, the annealing holding temperature is 800°C, the holding time is 4h, and the cooling rate is 3°C / min.
[0013] Preferably, in step 2, the thickness of the transition layer is 3.5 μm.
[0014] Preferably, in step three, the thickness of the Al2O3 insulating layer is 3 μm.
[0015] Preferably, the Solgel-Al2O3 obtained by the spin coating process in step 4 has a thickness of 2.5 μm.
[0016] Preferably, the spin coating speed in step 4 is 4000 rpm, the acceleration is 100 rpm / s, and the time is 120 s.
[0017] The technical effects of the present invention are:
[0018] According to the calculation results of diffusion kinetics and oxidation kinetics, in order to further improve the high-temperature electrical insulation of CVD-Al2O3 film (film obtained by high-temperature chemical vapor deposition), an effective method is to extend the diffusion path of Ti atoms, prepare a barrier layer on the surface of CVD-Al2O3 film, reduce the penetration of O2, increase the thickness of CVD-Al2O3, and use sol-gel solution to make a barrier layer and CVD-Al2O3 film to form a composite insulating film structure. The preparation of the composite film not only increases the thickness of the insulating film, but also introduces an interface barrier to reduce the diffusion of atoms such as Ti. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is the surface morphology and element analysis of the composite insulation layer and the side morphology and film distribution diagram of the composite insulation layer.
[0020] Figure 2 The graph shows the surface morphology changes of the composite film layer under different heat treatment temperatures.
[0021] Figure 3 Changes in the metal element content in the transition layer at different heat treatment temperatures.
[0022] Figure 4 X-ray diffraction analysis diagram of the composite insulating film layer prepared at different temperatures.
[0023] Figure 5 The surface morphology changes of 1.25μm thick CVD-Al2O3 at different temperatures.
[0024] Figure 6 These are X-ray diffraction test images of the surface of a 1.25μm thick CVD-Al2O3 film at different temperatures.
[0025] Figure 7 This is a characterization diagram of the morphology and properties of a 3.5μm thick CVD-Al2O3 film.
[0026] Figure 8 This is a diagram showing the changes in surface morphology and element content of 3.5μm thick CVD-Al2O3 film at different heat treatment temperatures.
[0027] Fig. 9 The surface morphology and element content changes of 3.5μm thick CVD-Al2O3 film under different heat treatment times.
[0028] Fig.10 These are X-ray diffraction test images of the surface of 3.5μm thick CVD-Al2O3 film at different temperatures.
[0029] Fig.11The surface morphology and element content changes of 3.5μm thick CVD-Al2O3 film at different temperatures. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with the accompanying drawings. The description in this part is only exemplary and explanatory and should not have any limiting effect on the protection scope of the present invention.
[0031] Example 1
[0032] A method for preparing a composite insulating film layer of a heat flow sensor for a bearing comprises the following steps:
[0033] Step 1: After mechanical grinding, GH3536 nickel-based high-temperature hard alloy is placed in a chemical reaction furnace;
[0034] Step 2: First, CH3CN (acetonitrile), TiCl4, etc. are used as the main reaction raw material gases to generate TiN and Ti(C,N) composite film layers at about 900°C as the transition layer of the nickel-based substrate thin film heat flow sensor. The thickness of the transition layer is 3.5μm, and the chemical reaction equation is:
[0035] TiCl4+CH3CN+H2+N2→Ti(C, N)+CH4+HCl
[0036] Step 3: AlCl3, H2 and CO2 are introduced to react at 1000°C to generate α-Al2O3 as an insulating layer with a thickness of 3 μm. The chemical reaction equation is:
[0037] 2AlCl3+3H2+3CO2→Al2O3+3CO+6HCl
[0038] Step 4: Spin-coat the surface of the Al2O3 film layer with an A-4-10 acidic aluminum sol-gel solution at a spin coating speed of 4000 rpm, an acceleration of 100 rpm / s, and a time of 120 s to prepare a 2.5 μm thick Sol-gel-Al2O3 barrier layer;
[0039] Step 5: annealing the composite film layer obtained in step 4, with an annealing heating rate of 2°C / min, an annealing holding temperature of 800°C, a holding time of 4h, and a cooling rate of 3°C / min to obtain a composite insulating film layer.
[0040] Comparative Examples 2-4
[0041] Compared with Example 1, Comparative Examples 2-4 are different only in the annealing and holding temperatures (i.e., heat treatment temperatures), which are 800°C, 850°C, 900°C, 950°C, and 1000°C for Example 1 and Comparative Examples 2-4, respectively.
[0042] The composite insulating layer obtained in Example 1 and Comparative Examples 2-4 was sampled and marked as samples E1, E2, E3, E4 and E5 respectively. The five samples were placed in a 950°C environment for 10 hours for evaluation. The changes in the surface metal element content of the evaluation group were compared with the preparation group to select the optimal annealing temperature. The SEM surface morphology of the preparation group and the evaluation group is shown in Figure 2. Figure 2 As shown in the figure, the EDS element test results of the film surface are as follows: Figure 3 As mentioned above, the experimental results show that when the annealing temperature exceeds 900°C, the content of diffused metal elements on the surface of the composite film layer will increase significantly. Therefore, the annealing temperature should be controlled within 900°C. According to the analysis results of diffused metal elements on the surface of the samples of the assessment group, the total content of diffused metal elements can be controlled within 2% for samples with an annealing temperature of less than 900°C during the preparation process. Considering that during the annealing process, the Ti atoms in the transition layer will diffuse into the alumina layer and the unformed barrier layer, the annealing temperature of 800°C is the best.
[0043] After the composite insulating film layer of Example 1 was prepared, it was kept at 950° C. for 2 h, 4 h, 6 h, 8 h and 10 h. The XRD analysis results of the film layer surface were as follows: Figure 4 As shown in the figure, the surface phase of the film layer is mainly composed of α-Al2O3 and a small amount of TiO2 and Ni3Al. The composite insulating film layer formed after the barrier layer is introduced has a phase composition that is extremely stable compared with the single CVD-Al2O3 film layer within 8 hours of heat preservation at 950℃. With the extension of the heat preservation time, the surface phase composition remains almost unchanged. After the heat preservation at 950℃ for more than 10 hours, a certain amount of TiO2 will be formed.
[0044] The XRD test results show that after introducing a barrier layer on the basis of the CVD-Al2O3 film layer, it can stably serve in a working environment of 950℃-1000℃ for a long time, which is suitable for the temperature environment of the heat flow sensor of the bearing.
[0045] Comparative Example 6 is an α-Al2O3 film layer with a thickness of 1.25 μm;
[0046] Comparative Example 7 is the optimized film layer of Comparative Example 6, which is an α-Al2O3 film layer with a thickness of 3.5 μm.
[0047] The GH3536 nickel-based alloy sample with a 1.25μm thick CVD-Al2O3 film was placed in a high-temperature tube furnace to characterize the surface properties of the film at different temperatures. The temperature of the tube furnace was raised to 550℃, 650℃, 750℃, 850℃ and 950℃ in turn and kept warm for 4 hours. The film at each temperature point was evaluated, and its surface was characterized by SEM and XRD to observe the changes in the content of metal elements in the transition layer on the surface of the alumina film and the alloy base, and to evaluate the maximum operating temperature of the 1.25μm thick α-Al2O3 film.
[0048] The surface morphology of the CVD-Al2O3 film layer of Comparative Example 6 after being kept at 550℃, 650℃, 750℃, 850℃ and 950℃ for 4 hours is as follows: Figure 5 The experimental results show that before 750℃, the surface of the aluminum oxide film is still dominated by tiny prism structures. When the temperature rises to 850℃, a large number of tetragonal prism structures appear on the surface of the film. When the test temperature exceeds 950℃, the prism structure on the surface of the film falls off.
[0049] After the CVD-Al2O3 film of Comparative Example 6 was heat treated at 550℃, 650℃, 750℃, 850℃ and 950℃ for 4h, the XRD analysis results of the oxide layer surface were as follows: Figure 6 As shown; the experimental results show that before 750℃, the CVD-Al2O3 film is mainly composed of α-Al2O3 and Ni3Al. From room temperature to 750℃, as the temperature increases, the surface phase composition remains almost unchanged. When the temperature exceeds 850℃, the composition of the phase on the film surface changes dramatically, and a region composed of tetragonal oblique prisms appears on the surface of the insulating layer, that is, a large amount of TiO2 phase is formed. When the temperature exceeds 950℃, the surface of the film begins to fall off due to the cyclic accumulation of temperature. Analyzing from the temperature at which TiO2 is formed, the temperature used for the CVD-Al2O3 film with a thickness of about 1.25μm cannot exceed 800℃.
[0050] The optimized CVD-Al2O3 film was placed in a high-temperature annealing furnace. The temperature of the annealing furnace was raised to 550℃, 650℃, 750℃, 850℃ and 950℃ in turn and kept warm for 4 hours. Compared with the film before optimization, the changes in the content of metal elements in the transition layer on the surface of the alumina film and the alloy substrate were observed, and the improvement effect of the surface properties and insulation of the optimized CVD-Al2O3 film in a high-temperature environment was evaluated.
[0051] The results of high temperature test show that the surface morphology of the film layer hardly changes within the temperature range of 550℃-950℃. Figure 8As shown in the figure, during the heating process, the diffusion coefficient of Ti atoms in the transition layer is low, and the content of Ti atoms on the surface of the film layer changes slightly. Compared with the 1.25μm-CVD-Al2O3 film layer, the increase in the thickness of the aluminum oxide film is conducive to reducing the precipitation of Ti atoms on the surface of the film layer, thereby widening the use temperature of the film layer.
[0052] After the CVD-Al2O3 optimized film layer was heat treated at 550℃, 650℃, 750℃, 850℃ and 950℃ for 4h, the XRD analysis results of the CVD-Al2O3 film layer surface were as follows: Fig.10 As shown in the figure, the surface phase of the film layer is mainly composed of α-Al2O3 and a small amount of TiO2 and Ni3Al. The experimental results show that the main surface phase of the CVD-Al2O3 optimized film layer is α-Al2O3 between 550℃ and 950℃. With the increase of temperature, the surface phase composition remains almost unchanged. Compared with the initial film layer, the α-Al2O3 diffraction peak shifts to the left. This is because the volume increase ratio of the oxide formed by the diffusion of a small amount of Ti atoms to the surface of the film layer causes the change of the lattice constant of alumina. The XRD test results show that the CVD-Al2O3 optimized film layer can stably serve in a working environment of 950℃.
[0053] The optimized film layer of Comparative Example 7, i.e., alloy samples D1, D2, D3, D4, and D5 with a thickness of 3.5 μm-CVD-Al2O3, were placed in a tubular quartz furnace, and the temperature of the quartz furnace was raised to 950°C at a rate of 3°C / min, and kept warm for 2h, 4h, 6h, 8h, and 10h, respectively. The surface of the 3.5 μm-thick CVD-Al2O3 film layer was characterized by SEM and XRD, and the changes in the surface morphology of the film layer and the content of the metal element Ti in the transition layer were observed, as shown in FIG. Fig. 9 As shown in the figure, the experimental results show that the Ti atom content on the surface of the optimized CVD-Al2O3 film is almost unchanged within 6 hours in a high temperature environment of 950℃. After the film is kept at a temperature of more than 6 hours, the Ti element content on the surface increases and narrow tetragonal prisms are produced. In addition, Cr atoms from the alloy substrate begin to appear. When the film is kept at a temperature of more than 10 hours, narrow tetragonal prisms begin to form in large quantities.
[0054] The XRD analysis results of the film surface after the CVD-Al2O3 optimized film structure was heat treated at 950℃ for 2h, 4h, 6h, 8h, and 10h are as follows: Fig.11As shown. The surface phase of the film layer is mainly composed of α-Al2O3 and a small amount of TiO2 and Ni3Al. The experimental results show that when the ambient temperature is 950°C, the heat treatment time of the CVD-Al2O3 film layer is less than 6 hours, its surface is mainly α-Al2O3, the TiO2 peak intensity is weak, and the surface phase composition is almost unchanged. When the heat treatment time exceeds 8 hours, a small amount of Ti atoms diffuse and precipitate to the surface of the film layer and react with O2, and the TiO2 diffraction peak begins to enhance, indicating that the optimized CVD-Al2O3 film layer can stably and for a long time (continuous 6 hours) serve in a 950°C working environment, which is much better than the CVD-Al2O3 film layer of Comparative Example 6.
[0055] Through the analysis and comparison of Example 1 and Comparative Example 7, it can be clearly concluded that the conforming film layer of Example 1 is more stable than the optimized film layer of Comparative Example 7, can stably serve in a working environment of 950°C-1000°C for a long time (at least continuously for 10 hours), and can be better adapted to the working environment of the bearing.
[0056] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0057] This article uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. The above is only a preferred implementation of the present invention. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, ordinary technicians in this technical field can make several improvements, modifications or changes without departing from the principles of the present invention, and can also combine the above technical features in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the inventive concept and technical solution to other occasions without improvement, should be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a composite insulating film layer for a heat flow sensor for a bearing, characterized in that: The steps include: Step 1: After mechanical grinding, GH3536 nickel-based high-temperature hard alloy is placed in a chemical reaction furnace; Step 2: First, CH3CN (acetonitrile), TiCl4, etc. are used as the main reaction raw material gases to generate TiN and Ti(C, N) composite film layers at about 900°C as the transition layer of the nickel-based substrate thin film heat flow sensor. The chemical reaction equation is: TiCl4+CH3CN+H2+N2→Ti(C, N)+CH4+HCl Step 3: AlCl3, H2 and CO2 are introduced to react at 1000°C to generate α-Al2O3 as an insulating layer. The chemical reaction equation is: 2AlCl3+3H2+3CO2→Al2O3+3CO+6HCl Step 4: Spin-coat the surface of the Al2O3 film layer with an A-4-10 acidic aluminum sol-gel solution to prepare a Sol-gel-Al2O3 barrier layer; Step 5: annealing the composite film layer obtained in step 4 to obtain a composite insulating film layer.
2. The method for preparing a composite insulating film layer of a thermal flow sensor for a bearing according to claim 1, characterized in that: In step 5, the annealing heating rate is 2°C / min, the annealing holding temperature is 800°C, the holding time is 4h, and the cooling rate is 3°C / min.
3. The method for preparing a composite insulating film layer of a thermal flow sensor for a bearing according to claim 1, characterized in that: In step 2, the thickness of the transition layer is 3.5 μm.
4. The method for preparing a composite insulating film layer of a thermal flow sensor for a bearing according to claim 3, characterized in that: In step 3, the thickness of the Al2O3 insulating layer is 3 μm.
5. The method for preparing a composite insulating film layer of a thermal flow sensor for a bearing according to claim 4, characterized in that: The thickness of Solgel-Al2O3 obtained by the spin coating process in step 4 is 2.5 μm.
6. The method for preparing a composite insulating film layer of a thermal flow sensor for a bearing according to claim 1, characterized in that: In step 4, the spin coating speed is 4000 rpm, the acceleration is 100 rpm / s, and the time is 120 s.