Method for modifying biological activity of titanium dioxide by utilizing nitrogen doping

The preparation of nitrogen-doped titanium dioxide nanotubes through anodization and high-temperature sublimation calcination solves the problem of insufficient antibacterial ability of titanium implants, achieves efficient photothermal antibacterial effects, and reduces the preparation cost.

CN118895543APending Publication Date: 2024-11-05SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310486803.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Titanium implants lack antibacterial ability in the field of oral implants, resulting in postoperative infection. The existing modification methods have limited effects and high cost of loading precious metal materials.

Method used

Titanium dioxide nanotubes were prepared on the titanium surface by anodizing and sublimated and calcined with melamine at high temperature in a nitrogen atmosphere to form nitrogen doped titanium dioxide nanotubes, enhancing their photothermal antibacterial properties.

Benefits of technology

It improves the photothermal conversion efficiency of the material, significantly kills bacteria, enhances antibacterial ability, and reduces preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a method for modifying titanium dioxide through nitrogen doping. Aiming at the problems of the titanium implant in clinical application, the titanium dioxide nanotube is generated by adopting an anodic oxidation process, the nitrogen-doped titanium dioxide nanotube is prepared by adopting a high-temperature calcination method, and experiments prove that the titanium dioxide nanotube shows good sterilization performance under the irradiation of near-infrared light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface modification of metal medical materials, and in particular relates to the preparation of titanium dioxide nanotube heterojunctions by means of anodic oxidation and nitrogen doping. Background Art

[0002] With the continuous development of medical materials, implantation has become the most effective way to solve tooth defects in the past seventy years. Among them, titanium implants are widely used in the field of oral implants due to their excellent mechanical properties and excellent corrosion resistance, but titanium lacks antibacterial ability and has a certain degree of biological inertness. In addition, postoperative infection of implant surgery is the main cause of implant failure. To solve the above problems, current research is on the one hand to modify the surface of titanium implants to enhance their biological activity, such as polishing, sandblasting, micro-arc oxidation (plasma spraying), laser cladding, acid etching, alkaline thermal reaction, anodizing, etc.; on the other hand, it is mainly to load a coating with antibacterial or osteogenic effects on the surface of titanium implants, thereby giving the implants antibacterial or osteogenic effects.

[0003] Anodizing is a mature treatment method for growing titanium dioxide nanotubes on the surface of titanium. By adjusting the composition of the electrolyte and the parameters of anodizing, porous titanium dioxide films of different sizes and roughness can be grown on the titanium surface. The thickness of the titanium dioxide film formed by anodizing is usually between a few nanometers and several hundred microns, and it has good adhesion and wear resistance.

[0004] Titanium nitride is a golden ceramic material with high hardness, high decomposition temperature and superconducting properties. Titanium nitride also has a plasma resonance effect. Titanium nitride can be combined with titanium dioxide to form a heterojunction, effectively broadening the light absorption range of titanium dioxide and achieving efficient light energy absorption through the plasma effect. In addition, the chemical properties of titanium nitride are extremely stable and still maintain good chemical stability at over 2000 °C. Compared with other precious metal materials, the advantages of combining titanium nitride with titanium dioxide are low preparation price and high economic benefits. Studies have shown that titanium nitride has certain photothermal conversion anti-cancer and bactericidal abilities. Summary of the invention

[0005] The purpose of the present invention is to provide a method for modifying titanium dioxide by nitrogen doping to improve biological activity, so as to prepare a material with excellent photothermal antibacterial properties.

[0006] To achieve the above object, the present invention adopts the following technical solution: Step 1, using a pure titanium sheet as an anode, and preparing titanium dioxide nanotubes on the surface of the pure titanium by an anodic oxidation method; Step 2: The obtained material is subjected to high-temperature sublimation calcination with melamine in a nitrogen atmosphere.

[0007] Furthermore, in the anodizing process, the anodizing voltage is 40-80 V, the anodizing is performed at room temperature for 10-30 min, and the electrolyte is an ethylene glycol solution of 0.1-0.4 M NH4F and 1-4 M H2O.

[0008] Furthermore, during high-temperature sublimation calcination, the mass of melamine is controlled to be 0.2-0.6 g, the distance between the titanium dioxide nanotubes and melamine is about 0.5-1.5 mm, the calcination time is 1-3 hours, the calcination temperature is controlled to be 650-850 °C, and the heating rate is 5-15 °C / min.

[0009] The advantages of the present invention are: Compared with the existing technology, the presence of titanium dioxide nanotubes on the surface of the implant can increase the surface roughness, which is beneficial for subsequent surface modification. Nitrogen is doped into titanium dioxide nanotubes to form titanium nitride crystals. The heterogeneous structure formed by the combination of titanium nitride and titanium dioxide can enhance the material's absorption of near-infrared light, and has excellent photothermal conversion efficiency, effectively killing bacteria. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 The SEM images of TiO2NTs prepared in Example 1 and the SEM images of N-TiO2NTs prepared in Example 2, Comparative Example 1 and Comparative Example 2.

[0011] Figure 2 The XRD diagrams of Example 1, Example 2, Comparative Example 1 and pure Ti are shown in FIG.

[0012] Figure 3 The present invention provides a thermal imaging diagram and a photothermal performance curve of the sample under near-infrared light irradiation.

[0013] Figure 4 This is the absorption curve and concentration change curve of RhB degradation of the sample provided by the present invention.

[0014] Figure 5 The photocurrent density of the sample provided by the present invention under light excitation of 450-600 nm.

[0015] Figure 6 This is a graph of the antibacterial experiment results provided by the present invention. DETAILED DESCRIPTION

[0016] In order to further illustrate the present invention, the following is a method for modifying the biological activity of titanium dioxide by nitrogen doping provided by the present invention in combination with examples. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

[0017] Example 1 First, the pure titanium sheet was ultrasonically treated in acetone, anhydrous ethanol and deionized water for 10 minutes in turn. At room temperature, NH4F / H2O / EG was used as the electrolyte (ethylene glycol solution containing 0.3 M NH4F and 3 M H2O), titanium was used as the anode, and platinum sheet was used as the cathode. Electrochemical oxidation was carried out for 20 minutes at room temperature, and the oxidation voltage was 60 V; after the oxidation, the sample was ultrasonically cleaned in anhydrous ethanol for 5 minutes, and after being soaked in anhydrous ethanol for 12 hours, it was dried with nitrogen. The material was named TiO2NTs.

[0018] Example 2 (1) Preparation of titanium dioxide nanotubes First, the pure titanium sheet was ultrasonically treated in acetone, anhydrous ethanol and deionized water for 10 min in sequence. At room temperature, NH4F / H2O / EG was used as the electrolyte (ethylene glycol solution containing 0.3 M NH4F and 3 M H2O), with metal titanium as the anode and platinum sheet as the cathode, and electrochemical oxidation was carried out for 20 min at an oxidation voltage of 60 V. After the oxidation, the sample was ultrasonically cleaned in anhydrous ethanol for 5 min, and then dried with nitrogen after being soaked in anhydrous ethanol for 12 h.

[0019] (2) Preparation of nitrogen-doped titanium dioxide nanotubes by high-temperature sublimation calcination Take 0.4g of melamine in a crucible, and fix the prepared titanium dioxide nanotubes upside down on top of the melamine, controlling the distance between the titanium dioxide nanotubes and the melamine to be 1 mm; in a nitrogen atmosphere, use a tubular furnace to calcine for 2 h, the calcination temperature is 750 °C, the heating rate is 10 °C / min, and the temperature is cooled to room temperature after calcination. The material is named N-TiO2NTs-1.

[0020] Comparative Example 1 Nitrogen-doped titanium dioxide nanotubes were prepared according to the method of Example 2, except that the calcination temperature in step (2) was 650° C. The material was named N-TiO2NTs-2.

[0021] Comparative Example 2 Nitrogen-doped titanium dioxide nanotubes were prepared according to the method of Example 2, except that the calcination temperature in step (2) was 850° C. The material was named N-TiO2NTs-3.

[0022] Test Case (1) Scanning electron microscopy observation of the surface morphology of the titanium dioxide nanotubes and nitrogen-doped titanium dioxide nanotubes prepared in Example 1: Figure 1 The average pore size of the titanium dioxide nanotubes is about 86.22 nm, which is conducive to subsequent surface modification. The calcination temperatures of Example 2 and Comparative Example 1 are 750°C and 650°C, respectively, and the resulting materials have regular morphology and uniform tube diameters; the calcination temperature of Comparative Example 2 is 850°C, and the resulting material has too thick tube walls and a destroyed tube structure, indicating that the temperature is too high.

[0023] (2) X-ray diffraction (XRD) was used to test Example 1, Example 2, Comparative Example 1 and pure Ti sample. The results are as follows: Figure 2 , obvious peaks of metallic titanium, anatase, and rutile phases can be observed in Example 2 and Comparative Example 1, and a cubic TiN peak can be observed in Example 2. In addition, between 35° and 40°, the peak of Example 2 shifts to the left relative to Example 1, which is the result that the atomic radius of nitrogen doped in N-TiO2NTs-1 is larger than that of lattice oxygen.

[0024] (3) Photothermal experiment of the nitrogen-doped titanium dioxide nanotube material prepared in Example 1 and Example 2 was carried out in 1 mL PBS buffer solution using 980 nm near-infrared light. 2 Infrared light was used as the irradiation source to detect the photothermal conversion performance of the sample and compare it with the pure Ti sample. Figure 4 : In the first two minutes, the N-TiO2NTs-1 sample had the highest heating rate. After 10 min of illumination, its temperature was higher than that of pure Ti and TiO2NTs samples, reaching a maximum of 46.5 °C, indicating that the N-TiO2NTs-1 prepared in Example 2 had the best photothermal performance.

[0025] (4) Rhodamine B (RhB) dye degradation experiment was used to evaluate the generation of active oxygen in Example 2 under near-infrared light: Example 1 was used as a blank control, and Example 1 and Example 2 were placed in a cuvette containing 8 mL 8 mg / L RhB dye, respectively, and fully mixed for 10 min under magnetic stirring to reach the adsorption equilibrium of the sample. The samples were subjected to near-infrared light at 980 nm and 300 mW / cm 2 The sample was irradiated with infrared light, and the dye absorbance was detected every 10 minutes using an ultraviolet spectrophotometer. Figure 5: After 10 min of adsorption, the absorbance of both groups of RhB dyes decreased, indicating that part of RhB was adsorbed by the nanotubes. After 30 min of illumination, the absorbance of the RhB dye solution in Example 2 decreased significantly, while the absorbance of the titanium dioxide nanotube dye prepared in Example 1 did not change significantly, indicating that the nitrogen-doped titanium dioxide nanotubes prepared in Example 2 can effectively generate reactive oxygen species under 980 nm NIR irradiation.

[0026] (5) The photocurrent density of the samples of Example 1 and Example 2 was detected by an electrochemical workstation to reflect the light response ability of the samples. The sample was used as the working electrode, the Pt electrode was used as the counter electrode, the saturated calomel electrode was used as the reference electrode, and the electrolyte was 0.1 M NaSO4 solution. In this experiment, the external bias voltage was controlled to be 0.5 V, and the photocurrent density of the sample was detected in the range of 450-600 nm (wavelength interval 10 nm). The experimental results are shown in Figure 2. Figure 6 : Under 450-600 nm light irradiation, the photocurrent density of the sample in Example 2 is greater than that of TiO2 with the same wavelength, indicating that nitrogen doping can enhance the light response ability of the nanotubes in the visible light range.

[0027] (6) The anti-Staphylococcus aureus ability of the samples of Example 1 and Example 2 was tested by the dilution plate method, and the samples were divided into three groups: Example 2, Example 2+NIR, and Example 1+NIR. In the culture medium, the cultivated Staphylococcus aureus and the samples were co-cultured at 37 °C for 24 h, then taken out, and the bacteria on the back of the material were killed with alcohol. The samples were then rinsed three times with PBS solution, and after being naturally dried, the illumination group was illuminated with 980 nm, 300 mW / cm 2 The surface of the nanotubes was irradiated with infrared light for 15 min and then ultrasonically treated. The non-irradiated group was placed for 15 min. After the irradiation, the sample was ultrasonically treated. The liquid obtained by ultrasonication was diluted 100 times and evenly spread on LB solid culture medium and cultured at 37 °C for 24 h. The experimental results are shown in Figure 6 : The illuminated N-TiO2NTs-1 sample showed obvious antibacterial effect compared with the non-illuminated N-TiO2NTs-1 sample, while the illuminated TiO2NTs and non-illuminated N-TiO2NTs-1 had no antibacterial effect.

Claims

1. A method for modifying the biological activity of titanium dioxide by nitrogen doping, characterized in that: Titanium dioxide nanotubes are prepared by anodization, and the microstructure of the composite material is optimized by controlling the temperature during nitrogen doping, so as to finally obtain nitrogen-doped titanium dioxide nanotube materials with improved biological activity, which have good bactericidal effect under 980nm near-infrared light irradiation; the preparation method of the material comprises the following steps: A pure titanium sheet is used as an anode and titanium dioxide nanotubes are prepared on the surface of the pure titanium by an anodic oxidation method; the obtained material is calcined with a nitrogen source to obtain nitrogen-doped titanium dioxide nanotubes.

2. A method for modifying the biological activity of titanium dioxide by nitrogen doping according to claim 1, characterized in that: The nitrogen source used for calcination is melamine.

3. A method for modifying the biological activity of titanium dioxide by nitrogen doping according to claim 1, characterized in that: The calcination adopts a high-temperature sublimation calcination method, specifically, the prepared titanium dioxide nanotubes are fixed on the top of the crucible with titanium wire, a small amount of melamine is taken into the crucible, and the distance between the titanium dioxide nanotubes and the melamine is controlled to be about 1 mm; under a nitrogen atmosphere, a tubular furnace is used for calcination for 2 h, and the calcination temperature is 750°C.

4. A method for modifying the biological activity of titanium dioxide by nitrogen doping according to claim 1, characterized in that: After high temperature sublimation calcination, nitrogen doping exists in the form of titanium nitride.