Moisture-absorption quick-dry high-power sunscreen breathable cool light and thin fabric and preparation method thereof

By blending titanium dioxide coated boron nitride with yarn raw materials, a breathable, cool and light fabric with high thermal conductivity, UV protection and moisture absorption and quick drying are prepared, which solves the problem of poor moisture absorption and sweating in summer, and achieves high-power sun protection The improvement of the cooling performance overcomes the shortcomings of insufficient uniform dispersion and thermal conductivity of boron nitride in the fiber.

CN118895573APending Publication Date: 2024-11-05WUXI CENTURY WIND FASHION CO LTD

Patent Information

Application Number
CN202410935672.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing UV-proof fabrics have poor moisture absorption and sweating properties when used in summer, resulting in stuffy and health problems. There are defects in the uniform dispersion and thermal conductivity of boron nitride in the fibers, affecting the coolness and sun protection performance of the fabric.

Method used

Use titanium dioxide-coated boron nitride to blend with yarn raw materials to prepare a breathable and cool thin fabric with high thermal conductivity, UV resistance and moisture absorption and quick drying properties through melt extrusion and spinning technology. It is coated with nitride by modified titanium dioxide-coated Boron improves fluidity and dispersion, enhancing the sun protection and coolness of the fabric.

Benefits of technology

It has achieved high-speed sun protection performance, excellent moisture absorption and quick drying properties and coolness. It has a weight of less than 100g/m2, providing lightweight comfort and excellent sun protection performance, far exceeding the national standard standards and is not weakened by long-term wear or washing. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895573A_ABST
    Figure CN118895573A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fabrics, and particularly discloses a moisture-absorption quick-dry high-power sunscreen breathable cool light and thin fabric and a preparation method thereof. Comprising the following steps: step 1, preparing titanium dioxide coated boron nitride; step 2: (1) uniformly mixing yarn raw materials, titanium dioxide coated boron nitride and ethylene-vinyl acetate, performing melt extrusion, cooling and pelletizing to obtain master batches; (2) fully drying the master batch, and performing melt spinning to obtain grey yarn; 3, weaving the grey yarn to form grey cloth; 4, the gray fabric is sequentially subjected to desizing, water washing, dyeing and sizing, and the breathable cool light and thin fabric is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabrics, and in particular to a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool and light fabric and a preparation method thereof. Background Art

[0002] Light is necessary for the normal growth and life of humans and the entire earth. Small doses of ultraviolet radiation are beneficial to the human body, helping bone development and sterilization. Excessive ultraviolet radiation can cause inflammation, sunburn, premature skin aging and other diseases, and even cause skin cancer. In recent years, environmental pollution has become increasingly serious, and the amount of ultraviolet light transmitted has increased day by day, which will inevitably cause more irreversible damage to the skin. Nowadays, people's health awareness is constantly improving, their life concepts are constantly changing, and they are paying more and more attention to outdoor activities. People spend more and more time outdoors and are more susceptible to the effects of solar radiation, especially in the summer when the sunshine is relatively strong. People use various cosmetics, sun hats, parasols and other sun protection measures to protect their skin, but these products are limited in terms of ultraviolet protection ability, action time and protection area, and have certain limitations. Therefore, textiles with large coverage and good sun protection ability have become the main means for people to protect themselves from the sun when traveling.

[0003] In the hot summer, conventional UV-proof fabrics can no longer meet people's needs. In order to reduce the feeling of heat, cool fabrics have become a consideration for people when choosing sunscreen products. Cool fabrics can quickly conduct the heat generated by the human body to the external environment. However, conventional cool fibers have poor moisture absorption and perspiration wicking properties, making it difficult to discharge sweat from the surface of the human body, causing a sense of stickiness between the human body and the fabric; in the hot summer or during high-intensity exercise, the skin sweats a lot. If the sweat cannot be discharged quickly, it will affect the conduction of vapor water, causing stuffiness and discomfort to the human body. At the same time, perspiration is also an effective cooling mechanism in a high temperature environment, but if the sweat cannot evaporate quickly, it will not only affect the cooling performance of the textile, but also have an impact on human health.

[0004] In the prior art, boron nitride is a highly thermally conductive filler with a graphite-like structure, and its thermal conductivity can reach 400w / m·K. It is blended with spinning raw materials to form a thermal conductive path inside the fiber to improve the thermal conductivity of the fiber, thereby achieving the cooling function of the fabric. However, simply adding boron nitride can easily lead to excessive viscosity of the polymer matrix when the boron nitride content is too high, which will affect the spinning properties of the yarn, and it also has other defects such as uniform dispersion. On the other hand, moisture absorption and quick drying are also one of the requirements for use in summer.

[0005] In summary, it is of great significance to solve the above problems and prepare a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool and lightweight fabric. Summary of the invention

[0006] The object of the present invention is to provide a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and light fabric and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric comprises the following steps:

[0009] Step 1: preparing titanium dioxide-coated boron nitride;

[0010] Step 2: (1) uniformly mixing yarn raw materials, titanium dioxide-coated boron nitride and ethylene-vinyl acetate, melt-extruding, cooling and pelletizing to obtain master batches; (2) fully drying the master batches, melt-spinning to obtain raw yarn;

[0011] Step 3: Weaving the raw yarn into grey fabric;

[0012] Step 4: Desizing, washing, dyeing and shaping the grey fabric in sequence to obtain a breathable, cool and light fabric.

[0013] More optimally, the preparation method of titanium dioxide-coated boron nitride comprises the following steps:

[0014] Polyvinyl pyrrolidone and boron nitride are added to ethanol in sequence, and stirred at 400-600 rpm for 2-4 hours; tetrabutyl titanate and acetylacetone are added, and stirred at room temperature for 12-16 hours, filtered, washed, and dried to obtain titanium dioxide-coated boron nitride.

[0015] More optimally, the raw materials of the titanium dioxide-coated boron nitride include the following components: by weight, 0.5-1.5 parts of polyvinyl pyrrolidone, 5-15 parts of boron nitride, 0.5-1.5 parts of tetrabutyl titanate, and 1-4 parts of acetylacetone; the ratio of boron nitride to ethanol is 5-15g:60-100mL.

[0016] More optimally, the mass ratio of the yarn raw material, titanium dioxide-coated boron nitride, and ethylene-vinyl acetate is 0.5-1.5:5-15:0.05-0.15; and the yarn raw material includes one or more of polyamide and polyester.

[0017] Preferably, in step 2 (1), the temperature of melt extrusion is 240-300°C;

[0018] In step 2 (2), during the melt spinning process: the screw temperature is 250-310°C, the spinning speed is 500-800 m / min, the drafting ratio is 2-4 times, and the spinneret shape is any one of a cross hole, 36 holes, and four-leaf shape; the temperature of the hot drafting roller is 70-120°C.

[0019] More optimally, the specification of the raw yarn is 20D-150D; the weaving structure of the grey cloth is any one of obvious check, hidden check, plain weave and twill.

[0020] Preferably, during the desizing process, the desizing method is cold batch desizing, the temperature is 80-90° C., the time is 20-30 hours, and the desizing liquid includes caustic soda and a degreasing agent;

[0021] During the water washing process, a low temperature-high temperature-low temperature method is adopted, the temperature is 80-120°C, the pressure is 10-20N, the vehicle speed is 20-40m / min, and the water washing liquid includes an emulsifier, a chelating agent and a dispersant;

[0022] During the dyeing process, a leveling agent is first added, the mixture is run at a low temperature of 25 to 35° C. for 10 to 20 minutes, and then half of the glacial acetic acid, dye and penetrant are added and run for 10 to 20 minutes; the temperature is raised to 60 to 80° C., and the remaining half of the glacial acetic acid is added and run for 15 to 25 minutes, the temperature is raised to a dyeing temperature of 95 to 130° C., and dyeing is performed for 30 to 50 minutes. After dyeing is completed, the mixture is cooled to 25 to 35° C. and then taken out of the vat for dehydration;

[0023] The dyeing temperature is generally set as follows: 120-130℃ for polyester fabric (the raw material is polyester chips), and 95-110℃ for nylon (the raw material is sliced ​​polyamide).

[0024] During the shaping process, the fabric is first placed in a finishing agent, double dipped and double rolled, dried at 80-110° C., and heat-set at 180-190° C. for 1-2 minutes.

[0025] In a further embodiment, the titanium dioxide-coated boron nitride is pre-modified and then melt-extruded with yarn raw material and ethylene-vinyl acetate to prepare a masterbatch; the process of pre-modification of the titanium dioxide-coated boron nitride is:

[0026] Step 1: Add vanillin to acetone, add dropwise an acetone solution of 2,4-dichloro-1,3,5-triazine under an ice bath, and stir for 1 to 2 hours; add dropwise a sodium carbonate solution, continue stirring for 1 to 2 hours, wash, and dry to obtain an anti-ultraviolet agent; add the solution to ethanol, add bis(2-aminoethyl) ether, react at 58 to 60° C. under a nitrogen atmosphere for 3 to 4 hours, remove the solvent, and purify to obtain an amino anti-ultraviolet agent;

[0027] Step 2: Mix titanium dioxide-coated boron nitride, ethanol, water, and epoxy silane coupling agent evenly, react at 60-65° C. for 10-12 hours, wash, and dry; place it in anhydrous ethanol, add amino anti-ultraviolet agent, stir at 60-70° C. for 24-36 hours under nitrogen atmosphere, wash, and dry to obtain modified titanium dioxide-coated boron nitride.

[0028] More optimally, the mass ratio of vanillin and 2,4-dichloro-1,3,5-triazine is 2:1; the mass ratio of the anti-UV agent and bis(2-aminoethyl) ether is 3:(2-2.2); the mass ratio of titanium dioxide-coated boron nitride, epoxy silane coupling agent, and amino anti-UV agent is 1:0.2:(0.4-0.5).

[0029] Preferably, the weight of the breathable, cool and light fabric is 70-100 g / m 2 .

[0030] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0031] (1) In order to reduce the matrix viscosity of the yarn raw material and increase the processing performance, the scheme improves the thermal conductivity while increasing other properties, such as UV resistance and moisture absorption and quick drying; titanium dioxide-coated boron nitride powder is successfully prepared by hydrolysis, and then blended with the spinning raw material, which can solve the problem of blending and spinning in the spinning solution to prepare raw yarn with cool feeling and UV protection. And because the fabric is raw yarn fabric, its sun protection and cool feeling will not decrease due to long-term wearing or increased number of washings. At the same time, the addition of boron nitride makes the fabric have better thermal conductivity, and it will not feel stuffy after wearing for a long time.

[0032] In addition, in a further scheme, titanium dioxide-coated boron nitride powder is modified; during the modification, an organic UV-resistant agent is prepared based on the reaction of hydroxyl and chlorine of vanillin and 2,4-dichloro-1,3,5-triazine, and then modified by the reaction of aldehyde group and amino group to obtain amino UV-resistant agent; finally, modified titanium dioxide-coated boron nitride is obtained by reaction grafting with amino group and epoxy group. The grafting of organic matter improves the fluidity of titanium dioxide-coated boron nitride in the yarn raw material and improves the dispersibility; and the presence of triazine group further synergistically improves the UV resistance of the original yarn; at the same time, due to the increase of hydrophilic groups such as ether bonds, the interfacial effect is improved while the moisture absorption and quick drying properties of the fabric are increased.

[0033] (2) The weight of the cool and light fabric prepared in the scheme is 100g / m 2 It is light and thin, which increases the lightness and comfort of the upper body; at the same time, in the weaving of the grey fabric, in addition to the plain and twill structures, two checkered structures are preferred. The checkered design makes the surface of the fabric have a texture, and at the same time makes the fabric more breathable and moisture-permeable when worn.

[0034] (3) The cool and light fabric prepared in the scheme has excellent sun protection performance, with an ultraviolet protection factor of 300+ and UVA less than 2%, far exceeding the national standard of 50+ and 5%, and has excellent moisture absorption and quick-drying performance. The fabric has a cool feeling performance, and the contact coolness coefficient Q-max value is above 0.24, far exceeding the national standard of 0.15. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0036] Figure 1 is a schematic diagram of the structure of the grey cloth with a clear checkered weaving structure in Example 1;

[0037] Figure 2 It is a schematic diagram of the grey cloth structure of the hidden grid weaving structure in Example 2. DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] In the following embodiments, it should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions, and exemplary examples include: the CAS number of vanillin is 121-33-5, the CAS number of 2,4-dichloro-1,3,5-triazine is 2831-66-5, and the CAS number of bis(2-aminoethyl) ether is 2752-17-2; the boron nitride is hexagonal boron nitride, CAS number 10043-11-5, purchased from Shenzhen Hongyuan Chemical New Material Technology Co., Ltd.; the model of polyamide chips is BL3280, purchased from Dongguan Hengyuyuan Engineering Plastics Co., Ltd.; the model of polyester chips is CZ3280, purchased from Shanghai Yunhongfu Plastics Co., Ltd. Co., Ltd.; the degreasing agent model is SX2100, purchased from Guangdong Sanxing High-tech Materials Technology Co., Ltd.; the emulsifier model is SX2100, purchased from Guangdong Sanxing High-tech Materials Technology Co., Ltd.; the chelating agent model is CF-A99, purchased from Foshan Chunfeng New Materials Technology Development Co., Ltd.; the dispersant model is NNO, purchased from Guangdong Sanxing High-tech Materials Technology Co., Ltd.; the leveling agent model is CF-YG02, purchased from Foshan Chunfeng New Materials Technology Development Co., Ltd.; the dye is disperse dye / acid dye, purchased from Zhejiang Longsheng Dye Chemical Co., Ltd.; the penetrant model is CF-GN1, purchased from Foshan Chunfeng New Materials Technology Development Co., Ltd.

[0040] Embodiment 1: A method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric, comprising the following steps:

[0041] Step 1: Preparation of titanium dioxide-coated boron nitride: 0.5 g polyvinyl pyrrolidone and 5 g boron nitride were added to 60 mL ethanol in sequence, and stirred at 400 rpm for 4 hours; 0.5 g tetrabutyl titanate and 1 g acetylacetone were added, and stirred at room temperature for 16 hours. After filtering and washing with ethanol several times, the mixture was dried in an oven at 80°C for 24 hours. After the powder was completely dried, high-power ultrasonic dispersion was used to break open the soft agglomerated particles produced during the drying process to obtain titanium dioxide-coated boron nitride with uniform particle size and an average particle size of 20 nm.

[0042] Step 2: (1) placing polyamide slices and titanium dioxide-coated boron nitride in a vacuum oven and drying them at 180° C. for 6 hours, then taking dispersant ethylene-vinyl acetate, the mass ratio of the three being 0.5:5:0.05, mixing the three evenly, adding them to a twin-screw for melt extrusion, the melting temperature being 240° C., and pelletizing them after cooling to obtain master batches; (2) placing the master batches in a blast drying oven, drying them at 120° C. for 4 hours, and using a spinning machine for melt spinning, the screw temperature being 250° C., the spinning speed being 500 m / min, the drafting multiple being 2 times, and the spinneret shape being a cross hole; the temperature of the hot drafting roller being 70° C., and obtaining raw yarns of different specifications, including 40D matte nylon FDY, 100D matte nylon DTY, and 70D matte nylon DTY;

[0043] Step 3: Weave the original yarn into grey fabric, which has a distinct checkered weaving structure. Figure 1 As shown, the complete weave includes 27 warp yarns and 23 weft yarns, the warp yarn density is 185 yarns / inch, and the weft yarn density is 135 yarns / inch; the warp yarn includes a first warp yarn and a second warp yarn, the first warp yarn is 40D matte nylon FDY, and the second warp yarn is 100D matte nylon DTY, the weft yarn includes a first weft yarn and a second weft yarn, the first weft yarn is 40D matte nylon FDY; the second weft yarn is 70D matte nylon DTY;

[0044] The arrangement of the first warp yarn and the second warp yarn is 3 second warp yarns and 24 first warp yarns, and the arrangement of the first weft yarn and the second weft yarn is 20 first weft yarns and 3 second weft yarns; 11 is the warp weave point, 22 is the weft weave point, and the structure of the warp and weft yarns interwoven in a complete weave is:

[0045] The first weft yarn is interwoven with the second, fourth, fifth, seventh, eighth, ninth, eleventh, twelfth, thirteenth, fifteenth, sixteenth, seventeenth, nineteenth, twenty-first, twenty-third, twenty-fourth, twenty-fifth, and twenty-seventh warp yarns to form warp points, and other warp yarns do not participate in the interweaving to form weft points;

[0046] The second weft yarn is interwoven with the first, third, fifth, sixth, ninth, tenth, thirteenth, fourteenth, seventeenth, eighteenth, twenty-first, twenty-second, twenty-fifth, and twenty-sixth warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0047] The third weft yarn is interwoven with the 2nd, 4th, 6th, 7th, 8th, 10th, 11th, 12th, 14th, 15th, 16th, 18th, 19th, 20th, 22nd, 23rd, 24th, 26th, and 27th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0048] The 4th weft yarn is interwoven with the 1st, 3rd, 5th, 7th, 9th, 11th, 13th, 15th, 17th, 19th, 21st, 23rd, 25th and 27th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0049] The 5th weft yarn is interwoven with the 2nd, 4th, 6th, 8th, 10th, 12th, 14th, 16th, 18th, 20th, 22nd, 24th and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0050] The 6th weft yarn is interwoven with the 1st, 3rd, 6th, 10th, 14th, 18th, 22nd and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0051] The 7th weft yarn is interwoven with the 2nd, 4th, 5th, 7th, 8th, 9th, 11th, 12th, 13th, 15th, 16th, 17th, 19th, 20th, 21st, 23rd, 24th, 25th, and 27th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0052] The 8th weft yarn is interwoven with the 1st, 3rd, 5th, 6th, 9th, 10th, 13th, 14th, 17th, 18th, 21st, 22nd, 25th, and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0053] The 9th weft yarn is interwoven with the 2nd, 4th, 6th, 7th, 8th, 10th, 11th, 12th, 14th, 15th, 16th, 18th, 19th, 20th, 22nd, 23rd, 24th, 26th, and 27th warp yarns to form warp points, and other warp yarns do not participate in the interweaving to form weft points;

[0054] The 10th weft yarn is interwoven with the 1st, 3rd, 5th, 7th, 9th, 11th, 13th, 15th, 17th, 19th, 21st, 23rd, 25th, and 27th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0055] The 11th weft yarn is interwoven with the 2nd, 4th, 6th, 8th, 10th, 12th, 14th, 16th, 18th, 20th, 22nd, 24th, and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0056] The 12th weft yarn is interwoven with the 1st, 3rd, 6th, 10th, 14th, 18th, 22nd, and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0057] The 13th weft yarn is interwoven with the 2nd, 4th, 5th, 7th, 8th, 9th, 11th, 12th, 13th, 15th, 16th, 17th, 19th, 20th, 21st, 23rd, 24th, 25th, and 27th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0058] The 14th weft yarn is interwoven with the 1st, 3rd, 5th, 6th, 9th, 10th, 13th, 14th, 17th, 18th, 21st, 22nd, 25th, and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0059] The 15th weft yarn is interwoven with the 2nd, 4th, 6th, 7th, 8th, 10th, 11th, 12th, 14th, 15th, 16th, 18th, 19th, 20th, 22nd, 23rd, 24th, 26th, and 27th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0060] The 16th weft yarn is interwoven with the 1st, 3rd, 5th, 7th, 9th, 11th, 13th, 15th, 17th, 19th, 21st, 23rd, 25th, and 27th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0061] The 17th weft yarn is interwoven with the 2nd, 4th, 6th, 8th, 10th, 12th, 14th, 16th, 18th, 20th, 22nd, 24th, and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0062] The 18th weft yarn is interwoven with the 1st, 3rd, 6th, 10th, 14th, 18th, 22nd, and 26th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0063] The 19th weft yarn is interwoven with the 2nd, 4th, 5th, 7th, 8th, 9th, 11th, 12th, 13th, 15th, 16th, 17th, 19th, 20th, 21st, 23rd, 24th, 25th, and 27th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0064] The 20th weft yarn is interwoven with the 1st, 3rd, 5th, 6th, 9th, 10th, 13th, 14th, 17th, 18th, 21st, 22nd, 25th, and 26th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0065] The 21st weft yarn is interwoven with the 3rd, 4th, 7th, 8th, 11th, 12th, 15th, 16th, 19th, 20th, 23rd, 24th, and 27th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0066] The 22nd weft yarn is interwoven with the 1st, 2nd, 5th, 9th, 13th, 17th, 21st, and 25th warp yarns to form warp weave points, and other warp yarns do not participate in interweaving to form weft weave points;

[0067] The 23rd weft yarn is interwoven with the 3rd, 6th, 7th, 10th, 11th, 14th, 15th, 18th, 19th, 22nd, 23rd, 26th, and 27th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0068] Step 4: Desizing the grey cloth in sequence: cold stack desizing, the desizing solution includes 15g / L caustic soda and 1.0g / L degreasing agent SX903A, the liquid temperature is 80℃, and the time is 20 hours; water washing: add 1.0g / L emulsifier SX2100, 1.5g / L chelating agent CF-A99 and 1.0g / L dispersant NNO into the water tank, set the main tank temperature to 80℃, set the low temperature-high temperature-low temperature principle, the pressure is 18N, and the speed is 20m / min; dyeing: first add 2g / L leveling agent CF-YG02, at low Run at 25℃ for 10min, then add half of 15g / L glacial acetic acid, acid dye and 2g / L penetrant, run for 10min; heat to 60℃, add the remaining half of 15g / L glacial acetic acid, run for 15min, heat to dyeing temperature 95℃, dye for 30min, cool to 25℃ after dyeing, take out of the cylinder for dehydration; shaping: put in the finishing agent containing 35g / L moisture absorption quick-drying finishing agent STA, double dip and double rolling, dry at 80℃, heat shaping at 180℃ for 1min; get breathable, cool and thin fabric, with a width of 140cm and a gram weight of 80g / m 2 .

[0069] Embodiment 2: A method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric, comprising the following steps:

[0070] Step 1: Preparation of titanium dioxide-coated boron nitride: Add 1g of polyvinyl pyrrolidone and 10g of boron nitride to 80mL of ethanol in turn, and stir at 500rpm for 3 hours; add 1g of tetrabutyl titanate and 2.5g of acetylacetone, stir at room temperature for 14 hours, filter and wash with ethanol several times, and then dry in an oven at 80℃ for 24 hours. After the powder is completely dried, use high-power ultrasonic dispersion to open the soft agglomerated particles produced during the drying process to obtain titanium dioxide-coated boron nitride with uniform particle size and an average particle size of 35nm.

[0071] Step 2: (1) placing polyamide slices and titanium dioxide-coated boron nitride in a vacuum oven and drying them at 150°C for 9 hours, then taking dispersant ethylene-vinyl acetate, the mass ratio of the three being 1:10:0.1, mixing the three evenly, adding them to a twin-screw for melt extrusion, the melting temperature being 270°C, and cutting into pellets after cooling to obtain master batches; (2) placing the master batches in a blast drying oven, drying them at 160°C for 5 hours, and using a spinning machine for melt spinning, the screw temperature being 280°C, the spinning speed being 650m / min, the drafting multiple being 3 times, and the spinneret shape being 36 holes; the temperature of the hot drafting roller being 100°C, and obtaining the raw yarn, the specification of which is 40D matte nylon DTY;

[0072] Step 3: Weave the original yarn into grey fabric, which has a hidden grid weaving structure. Figure 2 As shown, the complete weave includes 14 warp yarns and 10 weft yarns, the warp yarn density is 203 yarns / inch, and the weft yarn density is 130 yarns / inch;

[0073] The warp yarn is 40D matte nylon DTY, and the weft yarn includes a first weft yarn and a second weft yarn, wherein the first weft yarn is 40D matte nylon DTY, and the second weft yarn is two 40D matte nylon DTY yarns, and the arrangement of the first weft yarn and the second weft yarn is 7 first weft yarns and 3 second weft yarns;

[0074] A fully organized structure with warp and weft interlaced is:

[0075] The 1st, 2nd, 3rd, 4th, 5th, 6th, and 7th weft yarns are interwoven with the 3rd, 4th, 7th, 8th, 10th, and 12th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points; the 8th, 9th, and 10th weft yarns are interwoven with the 1st, 2nd, 5th, 6th, 9th, 11th, and 13th warp yarns to form warp points, and other warp yarns do not participate in interweaving to form weft points;

[0076] Step 4: Desizing the grey cloth in sequence: Desizing by cold stack desizing, the desizing liquid includes 25g / L caustic soda and 2.0g / L degreasing agent SX903A, the liquid temperature is 85℃, and the time is 25 hours; Water washing: Add 1.5g / L emulsifier SX2100, 1.5g / L chelating agent CF-A99 and 1.5g / L dispersant NNO into the water tank, set the main tank temperature to 100℃, set it by low temperature-high temperature-low temperature principle, the pressure is 19N, and the speed is 30m / min; Dyeing: First add 3g / L leveling agent CF-YG02, at low temperature Run at 30℃ for 15min, then add half of 20g / L glacial acetic acid, acid dye and 3g / L penetrant, run for 15min; heat to 70℃, add the remaining half of 20g / L glacial acetic acid, run for 20min, heat to dyeing temperature 98℃, dye for 40min, cool to 35℃ after dyeing, take out of the vat for dehydration; shaping: place in a finishing agent containing 45g / L moisture-absorbing quick-drying finishing agent STA, double dip and double rolling, dry at 100℃, heat set at 185℃ for 1.5min; get a breathable, cool and thin fabric with a width of 145cm and a gram weight of 70g / m 2 .

[0077] Embodiment 3: A method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric, comprising the following steps:

[0078] Step 1: Preparation of titanium dioxide-coated boron nitride: 1.5 g of polyvinyl pyrrolidone and 15 g of boron nitride were added to 100 mL of ethanol in sequence, and stirred at 600 rpm for 4 hours; 1.5 g of tetrabutyl titanate and 4 g of acetylacetone were added, and stirred at room temperature for 12 hours. After filtering and washing with ethanol several times, the mixture was dried in an oven at 80°C for 20 hours. After the powder was completely dried, high-power ultrasonic dispersion was used to break open the soft agglomerated particles produced during the drying process to obtain titanium dioxide-coated boron nitride with uniform particle size and an average particle size of 50 nm.

[0079] Step 2: (1) placing polyamide slices and titanium dioxide-coated boron nitride in a vacuum oven and drying them at 180°C for 6 hours, then taking dispersant ethylene-vinyl acetate, the mass ratio of the three being 1.5:15:0.15, mixing the three evenly, adding them to a twin-screw for melt extrusion, the melting temperature being 300°C, and pelletizing them after cooling to obtain master batches; (2) placing the master batches in a blast drying oven, drying them at 180°C for 4 hours, and using a spinning machine for melt spinning, the screw temperature being 310°C, the spinning speed being 800m / min, the drafting multiple being 4 times, and the spinneret shape being four-leaf; the temperature of the hot drafting roller being 120°C, and obtaining the raw yarn with a specification of 40D;

[0080] Step 3: Weaving the raw yarn into a grey fabric, the grey fabric has a plain weave structure, a warp yarn density of 180 yarns / inch, and a weft yarn density of 135 yarns / inch;

[0081] Step 4: Desizing the grey cloth in sequence: Desizing by cold stack desizing, the desizing liquid includes 35g / L caustic soda, 3.0g / L degreasing agent SX903A, the liquid temperature is 90℃, and the time is 20 hours; Water washing: Add 2g / L emulsifier SX2100, 2g / L chelating agent CF-A99 and 1.5g / L dispersant NNO into the water tank, set the main tank temperature to 120℃, set it by low temperature-high temperature-low temperature principle, the pressure is 18N, and the speed is 40m / min; Dyeing: First add 4g / L leveling agent CF-YG02, at low temperature 35 ℃ for 20 minutes, then add half of 30g / L glacial acetic acid, acid dye and 3.5g / L penetrant, and run for 20 minutes; heat up to 80℃, add the remaining half of 30g / L glacial acetic acid, and run for 25 minutes, heat up to dyeing temperature 110℃, dye for 30 minutes, and after dyeing, cool down to 35℃ and take out of the cylinder for dehydration; shaping: put in a finishing agent containing 55g / L of moisture-absorbing quick-drying finishing agent STA, double dip and double rolling, dry at 110℃, and heat set at 190℃ for 1 minute; obtain a breathable, cool and thin fabric with a width of 150cm and a gram weight of 90g / m 2 .

[0082] Embodiment 4: A method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric, comprising the following steps:

[0083] Step 1: Preparation of titanium dioxide-coated boron nitride: 1.2 g of polyvinyl pyrrolidone and 12 g of boron nitride were added to 80 mL of ethanol in sequence, and stirred at 500 rpm for 3 hours; 1 g of tetrabutyl titanate and 3 g of acetylacetone were added, and stirred at room temperature for 12 hours. After filtering and washing with ethanol several times, the mixture was dried in an oven at 70°C for 24 hours. After the powder was completely dried, high-power ultrasonic dispersion was used to break open the soft agglomerated particles produced during the drying process to obtain titanium dioxide-coated boron nitride with uniform particle size and an average particle size of 20 nm.

[0084] Step 2: (1) Place polyester chips and titanium dioxide-coated boron nitride in a vacuum oven and dry them at 160°C for 10 hours. Then take dispersant ethylene-vinyl acetate in a mass ratio of 1.5:15:0.15, mix the three evenly, add them into a twin-screw for melt extrusion at a melting temperature of 300°C, and cut into pellets after cooling to obtain master batches; (2) Place the master batches in a blast drying oven and dry them at 180°C for 4 hours. Use a spinning machine for melt spinning. The screw temperature is 310°C, the spinning speed is 800m / min, the drafting multiple is 4 times, and the spinneret shape is a cross hole; the temperature of the hot drafting roller is 120°C to obtain the raw yarn with a specification of 150D;

[0085] Step 3: Weaving the raw yarn into grey fabric, the grey fabric has a twill structure;

[0086] Step 4: Desizing the grey cloth in sequence: Desizing by cold stack desizing, the desizing liquid includes 35g / L caustic soda, 3.0g / L degreasing agent SX903A, the liquid temperature is 90℃, and the time is 20 hours; Water washing: Add 3g / L emulsifier SX2100, 3g / L chelating agent CF-A99 and 3g / L dispersant NNO into the water tank, set the main tank temperature to 120℃, set it by low temperature-high temperature-low temperature principle, the pressure is 20N, and the speed is 40m / min; Dyeing: First add 4g / L leveling agent CF-YG02, at a low temperature of 35℃ Run for 20 minutes, then add half of 30g / L glacial acetic acid, disperse dye and 4g / L penetrant, run for 20 minutes; heat to 80℃, add the remaining half of 30g / L glacial acetic acid, run for 25 minutes, heat to dyeing temperature 130℃, dye for 50 minutes, cool to 35℃ after dyeing, take out of the cylinder for dehydration; shaping: put in the finishing agent containing 55g / L moisture-absorbing quick-drying finishing agent STA, double dip and double rolling, dry at 110℃, heat set at 190℃ for 2 minutes; get a breathable, cool and thin fabric with a width of 150cm and a gram weight of 100g / m 2 .

[0087] Example 5: Based on Example 1, the titanium dioxide-coated boron nitride prepared therefrom is further modified, and the difference from Example 1 is that:

[0088] (1) 1.1: Place polyamide slices and titanium dioxide-coated boron nitride in a vacuum oven and dry at 180°C for 6 hours, then take dispersant ethylene-vinyl acetate and prepare the materials according to the mass ratio of the three being 0.5:5:0.05;

[0089] 1.2-1: Add 4g of vanillin to 10g of acetone, add dropwise an acetone solution of 2,4-dichloro-1,3,5-triazine (containing 2g of 2,4-dichloro-1,3,5-triazine and 10g of acetone) under an ice bath, and stir for 2 hours; add dropwise 2g of a 20wt% sodium carbonate solution, continue stirring for 1 hour, wash, and dry to obtain an anti-ultraviolet agent; add 3g of the anti-ultraviolet agent to 15g of ethanol, add 2.1g of bis(2-aminoethyl) ether, react at 60°C under a nitrogen atmosphere for 4 hours, remove the solvent, purify, and obtain an amino anti-ultraviolet agent, which can be scaled up in equal proportions;

[0090] 1.2-2: By weight, 1 part of titanium dioxide coated boron nitride, 40 parts of ethanol, 10 parts of water, and 0.2 parts of epoxy silane coupling agent KH-560 were mixed evenly, reacted at 62°C for 12 hours, washed and dried; the obtained powder was placed in 50 parts of anhydrous ethanol, 0.45 parts of amino anti-ultraviolet agent were added, stirred at 65°C for 24 hours under nitrogen atmosphere, washed and dried to obtain modified titanium dioxide coated boron nitride;

[0091] 2.1: Mix polyamide chips, modified titanium dioxide coated boron nitride and dispersant ethylene vinyl acetate evenly, add them into a twin screw for melt extrusion at a melting temperature of 240°C, and pelletize after cooling to obtain masterbatch;

[0092] (2) The masterbatch was placed in a blast drying oven and dried at 120° C. for 4 hours. The masterbatch was melt-spun using a spinning machine. The screw temperature was 250° C., the spinning speed was 500 m / min, the drafting ratio was 2 times, and the spinneret shape was a cross hole. The temperature of the hot drafting roller was 70° C. to obtain raw yarns of different specifications, including 40D matte nylon FDY, 100D matte nylon DTY, and 70D matte nylon DTY. The rest was the same as in Example 1.

[0093] Comparative Example 1: Woven fabric weight 90g / m 2 The fabric structure is plain weave, composition: polyamide, and the fabric is purchased on the market (Shaoxing Murray Textile Co., Ltd., model number is JY23351).

[0094] Comparative Example 2: Based on Example 5, the difference from Example 1 is that:

[0095] (1) 1.1: Place polyamide slices and titanium dioxide-coated boron nitride in a vacuum oven and dry at 180°C for 6 hours, then take dispersant ethylene-vinyl acetate and prepare the materials according to the mass ratio of the three being 0.5:5:0.05;

[0096] 1.2-1: Add 4 g of vanillin to 10 g of acetone, add dropwise an acetone solution of 2,4-dichloro-1,3,5-triazine (containing 2 g of 2,4-dichloro-1,3,5-triazine and 10 g of acetone) under an ice bath, and stir for 2 hours; add dropwise 2 g of a 20 wt% sodium carbonate solution, continue stirring for 1 hour, wash, and dry to obtain an anti-ultraviolet agent;

[0097] 1.2-2: By weight, 1 part of titanium dioxide coated boron nitride, 40 parts of ethanol, 10 parts of water, and 0.2 parts of aminosilane coupling agent KH-550 were mixed evenly, reacted at 62°C for 12 hours, washed and dried; the obtained powder was placed in 50 parts of anhydrous ethanol, 0.45 parts of anti-ultraviolet agent were added, stirred at 65°C for 24 hours under a nitrogen atmosphere, washed and dried to obtain modified titanium dioxide coated boron nitride;

[0098] 2.1: Polyamide chips, modified titanium dioxide coated boron nitride and dispersant ethylene vinyl acetate were mixed evenly, added into a twin screw for melt extrusion at a melting temperature of 240°C, and pelletized after cooling to obtain master batches; the rest was the same as in Example 5.

[0099] Performance test: The test standard for sun protection performance is GB / T18830-2009 "Evaluation of UV protection performance of textiles", the test standard for moisture absorption and quick-drying performance is GB / T21655.2-2019 "Evaluation of moisture absorption and quick-drying performance Part 2: Dynamic moisture transfer method"; the test standard for cooling performance is GB / T 35263-2017 "Testing and evaluation of instantaneous cooling performance of textiles"; the test standard for moisture permeability is GB / T12704.2-2009 "Test method for moisture permeability of textile fabrics Part 2: Evaporation method"; the test standard for air permeability is GB / T 5453-1997 "Determination of air permeability of textile fabrics"; the test results are shown in the following table:

[0100]

[0101]

[0102] Conclusion: It can be seen from the data in the above table that the breathable, cool and thin fabric prepared by the preparation method of the present invention has excellent sun protection performance, moisture absorption and quick-drying property, cool feeling performance and air permeability, which are significantly better than the fabric in Comparative Example 1. The comparative example does not have UV protection, moisture absorption and quick-drying property and cool feeling performance; at the same time, further modified titanium dioxide coated boron nitride can effectively improve the UV protection performance and moisture absorption and quick-drying property of the fabric.

[0103] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0104] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric, characterized in that: The following steps are involved: Step 1: preparing titanium dioxide-coated boron nitride; Step 2: (1) uniformly mixing yarn raw materials, titanium dioxide-coated boron nitride and ethylene-vinyl acetate, melt-extruding, cooling and pelletizing to obtain master batches; (2) fully drying the master batches, melt-spinning to obtain raw yarn; Step 3: Weaving the raw yarn into grey fabric; Step 4: Desizing, washing, dyeing and shaping the grey fabric in sequence to obtain a breathable, cool and light fabric.

2. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric according to claim 1, characterized in that: The preparation method of titanium dioxide-coated boron nitride comprises the following steps: Polyvinyl pyrrolidone and boron nitride are added to ethanol in sequence, and stirred at 400-600 rpm for 2-4 hours; tetrabutyl titanate and acetylacetone are added, and stirred at room temperature for 12-16 hours, filtered, washed, and dried to obtain titanium dioxide-coated boron nitride.

3. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric according to claim 1, characterized in that: The raw materials of titanium dioxide-coated boron nitride include the following components: by weight, 0.5-1.5 parts of polyvinyl pyrrolidone, 5-15 parts of boron nitride, 0.5-1.5 parts of tetrabutyl titanate, and 1-4 parts of acetylacetone; the ratio of boron nitride to ethanol is 5-15g:60-100mL.

4. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and light fabric according to claim 1, characterized in that: The mass ratio of the yarn raw material, titanium dioxide-coated boron nitride, and ethylene-vinyl acetate is 0.5-1.5:5-15:0.05-0.15; the yarn raw material includes one or more of polyamide and polyester.

5. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric according to claim 1, characterized in that: In step 2 (1), the temperature of melt extrusion is 240 to 300° C.; In step 2 (2), during the melt spinning process: the screw temperature is 250-310°C, the spinning speed is 500-800 m / min, the drafting ratio is 2-4 times, and the spinneret shape is any one of a cross hole, 36 holes, and four-leaf shape; the temperature of the hot drafting roller is 70-120°C.

6. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric according to claim 1, characterized in that: The specification of the raw yarn is 20D-150D; the weaving structure of the grey cloth is any one of obvious check, hidden check, plain weave and twill.

7. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric according to claim 1, characterized in that: In the desizing process, the desizing method is cold batch desizing, the temperature is 80-90° C., the time is 20-30 hours, and the desizing liquid includes caustic soda and a degreasing agent; During the water washing process, a low temperature-high temperature-low temperature method is adopted, the temperature is 80-120°C, the pressure is 10-20N, the vehicle speed is 20-40m / min, and the water washing liquid includes an emulsifier, a chelating agent and a dispersant; During the dyeing process, first add a leveling agent, operate at a low temperature of 25-35°C for 10-20 minutes, then add half of the glacial acetic acid, dye and penetrant, and operate for 10-20 minutes; heat up to 60-80°C, add the remaining half of the glacial acetic acid and operate for 15-25 minutes, heat up to the dyeing temperature of 95-130°C, dye for 30-50 minutes, and cool to 25-35°C after dyeing to remove from the cylinder for dehydration; during the setting process, first place in a finishing agent, double dip and double rolling, dry at 80-110°C, and heat set at 180-190°C for 1-2 minutes.

8. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and lightweight fabric according to claim 1, characterized in that: The titanium dioxide-coated boron nitride is pre-modified and then melt-extruded with yarn raw materials and ethylene-vinyl acetate to prepare a masterbatch; the process of pre-modification of the titanium dioxide-coated boron nitride is as follows: Step 1: Add vanillin to acetone, add dropwise an acetone solution of 2,4-dichloro-1,3,5-triazine under an ice bath, and stir for 1 to 2 hours; add dropwise a sodium carbonate solution, continue stirring for 1 to 2 hours, wash, and dry to obtain an anti-ultraviolet agent; add the solution to ethanol, add bis(2-aminoethyl) ether, react at 58 to 60° C. under a nitrogen atmosphere for 3 to 4 hours, remove the solvent, and purify to obtain an amino anti-ultraviolet agent; Step 2: Mix titanium dioxide-coated boron nitride, ethanol, water, and epoxy silane coupling agent evenly, react at 60-65° C. for 10-12 hours, wash, and dry; place it in anhydrous ethanol, add amino anti-ultraviolet agent, stir at 60-70° C. for 24-36 hours under nitrogen atmosphere, wash, and dry to obtain modified titanium dioxide-coated boron nitride.

9. The method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and light fabric according to claim 8, characterized in that: The mass ratio of vanillin to 2,4-dichloro-1,3,5-triazine is 2:1; the mass ratio of the anti-ultraviolet agent to bis(2-aminoethyl) ether is 3:(2-2.2); The mass ratio of titanium dioxide-coated boron nitride, epoxy silane coupling agent and amino anti-ultraviolet agent is 1:0.2:(0.4-0.5).

10. The breathable, cool, and light fabric prepared by the method for preparing a moisture-absorbing, quick-drying, highly sun-proof, breathable, cool, and light fabric according to any one of claims 1 to 9 is characterized in that: The weight of the breathable, cool and light fabric is 70-100 g / m 2 .

Citation Information

Patent Citations

  • Heat-conducting cool-feeling, moisture-absorbing and sweat-releasing polyamide fiber material and preparation method thereof

    CN111172608A

  • Nano SiO2 coated BN composite powder, preparation method thereof and thermal conductive material

    CN111534287A

  • Cool nylon blend and application thereof

    CN115124831A

  • Modified kaolinite reinforced flame-retardant waste resin composite material and preparation method thereof

    CN116178843A

  • UV Light Protective Fiber and Fabric having Refrigerant Performance

    KR101960080B1

Cited By