High-strength chinlon filament and preparation method thereof

By employing three-layer interlaced spiral winding and freeze-spun technology, the problem of insufficient strength of nylon filaments during blending was solved, improving overall performance and surface smoothness.

CN118895589APending Publication Date: 2024-11-05FUJIAN KAIBANG POLYAMIDE TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411190342.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing nylon filaments exhibit reduced performance when blended with other fibers, resulting in insufficient strength and easy breakage.

Method used

The material is made by spirally winding two bundles of nylon filaments and one bundle of polypropylene fiber filaments in an alternating manner, with three layers of rings interwoven. The outer layer of nylon filaments, the middle layer of polypropylene fiber filaments, and the inner layer of nylon filaments are bonded together. Low-temperature cold drawing and heat treatment are carried out in combination with cryogenic textile technology.

Benefits of technology

It significantly improves the overall strength and modulus of nylon filament, maintains the original properties of nylon filament, and makes the fabric surface smooth and beautiful.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a high-strength chinlon filament and a preparation method thereof, and relates to the technical field of textile chemical fibers. The high-strength chinlon filament comprises two bundles of chinlon yarns and one bundle of polypropylene fiber yarns which are wound in an internal and external staggered and mutually spiral mode, the chinlon yarns and the polypropylene fiber yarns are distributed in a three-layer annular staggered mode, the chinlon yarns on the outer layer are distributed in an annular mode, the polypropylene fiber yarns on the middle layer are distributed in an annular mode, and the chinlon yarns on the inner layer are a main core; the diameter of the nylon yarns on the outer layer is 0.03-0.08 mm, and the number of the nylon yarns on the outer layer is 8-12; the diameter of the polypropylene fiber yarns in the middle layer is 0.05-0.08 mm, and the number of the polypropylene fiber yarns in the middle layer is 3-5. Through the structure, the polyamide yarns and the polypropylene fiber yarns are arranged and combined in a special arrangement mode, so that physical winding is carried out under the condition that the purity of the polyamide yarns is not reduced, all good characteristics of the polyamide yarns are reserved, and the polyamide yarns are further enhanced under the promotion of the polypropylene fiber yarns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile chemical fibers, and in particular to a high-strength nylon filament and a preparation method thereof. Background Art

[0002] Nylon filament, also known as polyamide fiber, is a widely used synthetic fiber that has a wide range of applications in many fields due to its unique physical and chemical properties. From clothing, outdoor equipment to medical supplies, to home decoration, the use of nylon filament covers almost every aspect of people's lives. Its wear resistance, high strength and good elasticity make nylon filament the material of choice for many designers and manufacturers.

[0003] Although nylon filaments have outstanding performance in terms of wear resistance, strength and elasticity, the existing nylon filaments have very small diameters and are often blended with other fibers, resulting in reduced performance. In addition, the too small diameter further causes the nylon filaments to be insufficient in strength and easy to break. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides a high-strength nylon filament and a preparation method thereof, which solves the problem that the performance of nylon filament is reduced due to blending with other fibers, and the small diameter of the blended fibers further reduces the performance of nylon filament and causes the nylon filament to be easily broken.

[0006] (II) Technical solution

[0007] To achieve the above objectives, the present invention is implemented through the following technical scheme: a high-strength nylon filament, including two bundles of nylon yarns and a bundle of polypropylene fiber yarns, which are interlaced and spirally wound inside and outside, and the nylon yarns and polypropylene fiber yarns are distributed in three layers in an annular and staggered manner, the nylon yarns in the outer layer are distributed in an annular manner, the polypropylene fiber yarns in the middle layer are distributed in an annular manner, and the nylon yarns in the inner layer are the main core.

[0008] Preferably, the diameter of the nylon yarn in the outer layer is 0.03-0.08 mm, and the number of the nylon yarns in the outer layer is 8-12.

[0009] Preferably, the diameter of the polypropylene fiber filaments in the middle layer is 0.05-0.08 mm, and the number of the polypropylene fiber filaments in the middle layer is 3-5.

[0010] Preferably, the diameter of the nylon yarn in the inner layer is 0.08-0.12 mm, and the number of the nylon yarn in the inner layer is one.

[0011] Preferably, the mass ratio of the nylon yarn to the polypropylene fiber yarn is 17:3.

[0012] A method for preparing high-strength nylon filaments comprises the following preparation steps:

[0013] S1, subjecting adipic acid and hexamethylenediamine to polycondensation reaction under high temperature and high pressure conditions to generate a polyamide melt, and then spraying the generated polyamide melt into nylon yarn through a spinneret;

[0014] S2, mixing the polypropylene resin and the additive uniformly and feeding the mixture into an extruder to extrude polypropylene fiber filaments;

[0015] S3, arranging the nylon yarn and the polypropylene fiber yarn inside and outside, with the outer layer being the nylon yarn, the middle layer being the polypropylene fiber yarn, and the inner layer being the nylon yarn, and making the outer layer nylon yarn, the middle layer polypropylene fiber yarn, and the inner layer nylon yarn interlaced and spirally wound with each other;

[0016] S4, sending the arranged mixed yarns into a hot oven for heating, and further performing spiral twisting during the heating process to make the nylon yarn and the polypropylene fiber layers closely adhere to each other, and performing roller-type surface treatment during the spiral twisting process to make the surface of the mixed yarn smooth, so that the multiple nylon yarns in the outer layer are bonded to each other, forming protection inside and making the outside smoother and more beautiful;

[0017] S5, low-temperature stretching the heat-treated silk thread to further refine it, stretching the mixed silk thread to a nylon filament that meets the requirements, and adopting a freezing textile technology to perform low-temperature cold drawing. The low-temperature cold drawing process in the freezing textile technology can obtain highly oriented and highly crystalline fibers, significantly improving the overall strength and modulus of the nylon filament;

[0018] S6, heat-treating the silk thread after low-temperature stretching, the second heat treatment can shape the blended nylon filaments and further improve the performance of the nylon filaments;

[0019] S7. Finally, the heat-treated silk thread is cooled, cleaned, dried and rolled up.

[0020] Preferably, the nylon yarn in S1 and the polypropylene fiber yarn in S2 are both preliminarily formed yarns. The diameter of the yarns obtained at this time is much larger than the diameter of the formed yarns, which is convenient for subsequent yarn arrangement, winding and heat treatment.

[0021] Preferably, the heating is performed by hot air supply in S4. The heating can be performed more evenly and quickly by hot air supply.

[0022] Preferably, the low-temperature cold drawing is performed by using a freezing spinning technique in S6. The low-temperature cold drawing process in the freezing spinning technique can obtain highly oriented and highly crystalline fibers, significantly improving the overall strength and modulus of the nylon filaments.

[0023] Preferably, ethanol is used for sealed cleaning in S7, and the wire is dried in a sealed container to remove contamination on the wire surface during the preparation process.

[0024] (III) Beneficial effects

[0025] The present invention provides a high-strength nylon filament and a preparation method thereof. The present invention has the following beneficial effects:

[0026] 1. The present invention arranges and combines nylon yarn and polypropylene fiber yarn in a special arrangement mode, thereby performing physical entanglement without reducing the purity of nylon yarn, which not only retains all the good properties of nylon yarn itself, but also further enhances them with the promotion of polypropylene fiber yarn.

[0027] 2. When the mixed yarn is subjected to the first heat treatment, the outer layer, the middle layer and the inner layer of the yarn are more tightly bonded and more evenly stressed through spiral winding, which has a good promoting effect on enhancing the overall performance of the nylon filament.

[0028] 3. The present invention adopts the cold drawing process in the freezing textile technology when stretching the mixed yarn, so as to obtain highly oriented and highly crystalline fibers, and significantly improve the overall strength and modulus of the nylon filaments. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] An embodiment of the present invention provides a high-strength nylon filament, comprising two bundles of nylon yarns and a bundle of polypropylene fiber yarns, which are interlaced and wound in a spiral manner. The nylon yarns and the polypropylene fiber yarns are distributed in three layers in an annular and interlaced manner, the outer layer of nylon yarns are distributed in an annular manner, the middle layer of polypropylene fiber yarns are distributed in an annular manner, the inner layer of nylon yarns is a main core, the diameter of the outer layer of nylon yarns is 0.03-0.08mm, the number of the outer layer of nylon yarns is 8-12, the diameter of the middle layer of polypropylene fiber yarns is 0.05-0.08mm, the number of the middle layer of polypropylene fiber yarns is 3-5, the diameter of the inner layer of nylon yarns is 0.08-0.12mm, the number of the inner layer of nylon yarns is one, and the mass ratio of nylon yarns to polypropylene fiber yarns is 17:3.

[0032] The three-layer structure uses nylon yarn, polypropylene fiber yarn and nylon yarn in turn. The polypropylene fiber yarn in the middle is a composite material for reinforcing nylon filament yarn. Polypropylene fiber is the lightest chemical fiber and also has high strength, high elasticity and high wear resistance, similar to the performance of nylon yarn. The combination of the two can improve the overall performance of nylon yarn. At the same time, the mass ratio of nylon yarn to polypropylene fiber yarn is 17:3, which can also reduce the weight of nylon filament yarn per unit volume.

[0033] Moreover, the three-layer structure adopts an inside-outside staggered spiral distribution, which is structurally superior and can make the internal stress of the nylon filament more dispersed and the force more evenly distributed, which has a good promoting effect on the overall performance of the nylon filament. The inner layer of nylon yarn has the largest diameter and can stabilize the main body of the silk thread. The outer layer of nylon yarn has the smallest diameter and the largest number, making the overall surface of the nylon filament smoother.

[0034] The three-layer structure is thermally bonded inside and outside. During the thermal bonding, the three-layer structure spirally rotates. This connection method increases the thermal bonding area between the inside and outside, thereby having better stability and avoiding the phenomenon of single yarn derailment. At the same time, it avoids the use of adhesives. Adhesives are additives that will also reduce the overall performance of nylon filaments. During the spiral twisting process, roller-type surface treatment is simultaneously performed to make the surface of the mixed yarn smooth and make the multiple nylon yarns in the outer layer bonded to each other, forming protection inside and making it smoother and more beautiful outside.

[0035] A method for preparing high-strength nylon filaments comprises the following preparation steps:

[0036] S1, polycondensing adipic acid and hexamethylenediamine under high temperature and high pressure to generate a polyamide melt, and then spraying the generated polyamide melt into nylon yarn through a spinneret, first preparing the nylon yarn, and then keeping it for subsequent production use after completion. At this time, the diameter of the nylon yarn is much larger than the final diameter of the nylon filament;

[0037] S2, mixing the polypropylene resin and the additives uniformly and feeding them into an extruder to extrude polypropylene fiber filaments, and then preparing the polypropylene fiber filaments, and then keeping them for subsequent production use. At this time, the diameter of the polypropylene fiber filaments is much larger than the final diameter of the nylon filaments;

[0038] S3, arranging nylon yarn and polypropylene fiber yarn inside and outside, with the outer layer being nylon yarn, the middle layer being polypropylene fiber yarn, and the inner layer being nylon yarn, and making the outer layer nylon yarn, the middle layer polypropylene fiber yarn, and the inner layer nylon yarn interlaced and spirally wound with each other, and the special distribution can improve the performance of the final nylon filament yarn;

[0039] S4, sending the arranged mixed yarns into a hot oven for heating, and further performing spiral twisting during the heating process to make the nylon yarn and the polypropylene fiber layers adhere closely to each other, and performing roller-type surface treatment during the spiral twisting process to make the surface of the mixed yarn smooth, so that the multiple nylon yarns in the outer layer adhere to each other, forming protection inside and making the outside smoother and more beautiful. The first heat treatment adopts hot air supply method for heating, and the hot air supply method for heating can make the heating more uniform and rapid;

[0040] S5, low-temperature stretching the heat-treated silk thread to further refine it, stretching the mixed silk thread to a nylon filament that meets the requirements, and adopting a freezing textile technology to perform low-temperature cold drawing. The low-temperature cold drawing process in the freezing textile technology can obtain highly oriented and highly crystalline fibers, significantly improving the overall strength and modulus of the nylon filament;

[0041] S6, heat-treating the silk thread after low-temperature stretching, the second heat treatment can shape the blended nylon filaments and further improve the performance of the nylon filaments;

[0042] S7. Finally, the heat-treated silk thread is cooled, cleaned, dried, and rolled up to remove impurities attached to the nylon filaments during the preparation process, and then stored.

[0043] The nylon yarn in S1 and the polypropylene fiber yarn in S2 are both preliminarily formed yarns.

[0044] In S7, ethanol was used for sealing and cleaning, and the wire was dried in a sealed container to remove surface contamination during the preparation process.

[0045] Comparative Example 1:

[0046] An embodiment of the present invention provides a high-strength nylon filament, comprising two bundles of nylon yarns and a bundle of polypropylene fiber yarns, which are staggered inside and outside. The nylon yarns and the polypropylene fiber yarns are staggered in three layers, the nylon yarns in the outer layer are distributed in a ring shape, the polypropylene fiber yarns in the middle layer are distributed in a ring shape, the nylon yarns in the inner layer are the main core, the diameter of the outer layer nylon yarn is 0.03-0.08mm, the number of the outer layer nylon yarns is 8-12, the diameter of the middle layer polypropylene fiber yarn is 0.05-0.08mm, the number of the middle layer polypropylene fiber yarn is 3-5, the diameter of the inner layer nylon yarn is 0.08-0.12mm, the number of the inner layer nylon yarn is one, and the mass ratio of nylon yarn to polypropylene fiber yarn is 17:3.

[0047] A method for preparing high-strength nylon filaments comprises the following preparation steps:

[0048] S1, polycondensing adipic acid and hexamethylenediamine under high temperature and high pressure to generate a polyamide melt, and then spraying the generated polyamide melt into nylon yarn through a spinneret, first preparing the nylon yarn, and then keeping it for subsequent production use after completion. At this time, the diameter of the nylon yarn is much larger than the final diameter of the nylon filament;

[0049] S2, mixing the polypropylene resin and the additives uniformly and feeding them into an extruder to extrude polypropylene fiber filaments, and then preparing the polypropylene fiber filaments, and then keeping them for subsequent production use. At this time, the diameter of the polypropylene fiber filaments is much larger than the final diameter of the nylon filaments;

[0050] S3, arranging the nylon yarn and the polypropylene fiber yarn inside and outside, the outer layer is the nylon yarn, the middle layer is the polypropylene fiber yarn, and the inner layer is the nylon yarn, and the outer layer nylon yarn, the middle layer polypropylene fiber yarn, and the inner layer nylon yarn are staggered inside and outside, and the special distribution can improve the performance of the final nylon filament;

[0051] S4, sending the arranged mixed yarns into a hot oven for heating, and performing roller-pressing surface treatment during the heating process to make the surface of the mixed yarn smooth, and to make the nylon yarn and the polypropylene fiber yarn layers adhere closely to each other, so that multiple nylon yarns in the outer layer are bonded to each other, forming protection inside and making the outside smoother and more beautiful. The first heat treatment adopts hot air supply method for heating, and the hot air supply method for heating can make the heating more uniform and rapid;

[0052] S5, low-temperature stretching the heat-treated silk thread to further refine it, stretching the mixed silk thread to a nylon filament that meets the requirements, and adopting a freezing textile technology to perform low-temperature cold drawing. The low-temperature cold drawing process in the freezing textile technology can obtain highly oriented and highly crystalline fibers, significantly improving the overall strength and modulus of the nylon filament;

[0053] S6, heat-treating the silk thread after low-temperature stretching, the second heat treatment can shape the blended nylon filaments and further improve the performance of the nylon filaments;

[0054] S7. Finally, the heat-treated silk thread is cooled, cleaned, dried, and rolled up to remove impurities attached to the nylon filaments during the preparation process, and then stored.

[0055] The nylon yarn in S1 and the polypropylene fiber yarn in S2 are both preliminarily formed yarns.

[0056] In S7, ethanol was used for sealing and cleaning, and the wire was dried in a sealed container to remove surface contamination during the preparation process.

[0057] Comparative Example 2:

[0058] A high-strength nylon filament comprises a nylon yarn and a polypropylene fiber yarn which are wound in a spiral manner, and the mass ratio of the nylon yarn to the polypropylene fiber yarn is 17:3.

[0059] A method for preparing high-strength nylon filaments comprises the following preparation steps:

[0060] S1, subjecting adipic acid and hexamethylenediamine to polycondensation reaction under high temperature and high pressure conditions to generate a polyamide melt, and then spraying the generated polyamide melt into nylon yarn through a spinneret;

[0061] S2, mixing the polypropylene resin and the additive uniformly and feeding the mixture into an extruder to extrude polypropylene fiber filaments;

[0062] S3, arranging a single nylon yarn and a single polypropylene fiber yarn left and right, and entwining them with each other;

[0063] S4, sending the arranged mixed silk threads into a hot oven for heating, and performing roller-type surface treatment during the heating process to make the surface of the mixed silk threads smooth and make the nylon silk and polypropylene fiber layers closely adhered to each other, and performing roller-type surface treatment during the spiral twisting process to make the surface of the mixed silk threads smooth and more beautiful;

[0064] S5, low-temperature stretching the heat-treated silk thread to further refine it, stretching the mixed silk thread to a nylon filament that meets the requirements, and adopting a freezing textile technology to perform low-temperature cold drawing. The low-temperature cold drawing process in the freezing textile technology can obtain highly oriented and highly crystalline fibers, significantly improving the overall strength and modulus of the nylon filament;

[0065] S6, heat-treating the silk thread after low-temperature stretching, the second heat treatment can shape the blended nylon filaments and further improve the performance of the nylon filaments;

[0066] S7. Finally, the heat-treated silk thread is cooled, cleaned, dried, and rolled up to remove impurities attached to the nylon filaments during the preparation process, and then stored.

[0067] The nylon yarn in S1 and the polypropylene fiber yarn in S2 are both preliminarily formed yarns.

[0068] In S7, ethanol was used for sealing and cleaning, and the wire was dried in a sealed container to remove surface contamination during the preparation process.

[0069] The composite yarn was woven into fabrics by the methods of Example 1, Comparative Example 1 and Comparative Example 2, and the three fabrics were tested by a fabric testing instrument, and the test results were compared. The comparison results are shown in Table 1:

[0070] Table 1

[0071] Embodiment 1 Comparative Example 1 Comparative Example 2 Number of layers Three layers inside and outside Three layers inside and outside Single layer Arrangement Spiral interlacing Ring staggered Double wire winding Performance Strength powerful good generally Surface smoothness smooth smooth Rough

[0072] From the results in Table 1, it can be seen that after the nylon filaments prepared by the inner and outer three-layer staggered spiral winding method in Example 1 are made into cloth, the performance strength of the cloth is significantly enhanced, and the surface of the cloth is smoother. After the nylon filaments prepared by the inner and outer three-layer annular staggered method in Comparative Example 1 are made into cloth, although the surface of the cloth is smooth, the performance strength is not significantly enhanced. After the nylon filaments prepared by the double-wire winding method in Comparative Example 2 are made into cloth, the performance strength of the cloth is general and the surface of the cloth is relatively rough.

[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength nylon filament, characterized in that: It comprises two bundles of nylon yarns and one bundle of polypropylene fiber yarns which are interlaced and wound in a spiral manner. The two bundles of nylon yarns and the one bundle of polypropylene fiber yarns are distributed in three layers in an annular and interlaced manner. The nylon yarns in the outer layer are distributed in an annular manner, the polypropylene fiber yarns in the middle layer are distributed in an annular manner, and the nylon yarns in the inner layer are the main core.

2. The high-strength nylon filament according to claim 1, characterized in that: The diameter of the nylon yarn in the outer layer is 0.03-0.08 mm, and the number of the nylon yarn in the outer layer is 8-12.

3. The high-strength nylon filament according to claim 1, characterized in that: The diameter of the polypropylene fiber filaments in the middle layer is 0.05-0.08 mm, and the number of the polypropylene fiber filaments in the middle layer is 3-5.

4. The high-strength nylon filament according to claim 1, characterized in that: The diameter of the nylon yarn in the inner layer is 0.08-0.12 mm, and the number of the nylon yarn in the inner layer is one.

5. The high-strength nylon filament according to claim 1, characterized in that: The mass ratio of the nylon yarn to the polypropylene fiber yarn is 17:

3.

6. A method for preparing high-strength nylon filament, based on the high-strength nylon filament according to any one of claims 1 to 5, comprising the following preparation steps: S1, subjecting adipic acid and hexamethylenediamine to polycondensation reaction under high temperature and high pressure conditions to generate a polyamide melt, and then spraying the generated polyamide melt into nylon yarn through a spinneret; S2, mixing the polypropylene resin and the additive uniformly and feeding the mixture into an extruder to extrude polypropylene fiber filaments; S3, arranging the nylon yarn and the polypropylene fiber yarn inside and outside, with the outer layer being the nylon yarn, the middle layer being the polypropylene fiber yarn, and the inner layer being the nylon yarn, and making the outer layer nylon yarn, the middle layer polypropylene fiber yarn, and the inner layer nylon yarn interlaced and spirally wound with each other; S4, sending the arranged mixed yarns into a hot oven for heating, and further performing spiral twisting during the heating process to make the nylon yarn and the polypropylene fiber layers adhere closely to each other, and performing roller-type surface treatment during the spiral twisting process to make the surface of the mixed yarn smooth; S5, stretching the heat-treated silk thread at low temperature to further refine it; S6, heat treating the silk thread after low-temperature stretching; S7. Finally, the heat-treated silk thread is cooled, cleaned, dried and rolled up.

7. The method for preparing high-strength nylon filament according to claim 6, characterized in that: The nylon yarn in S1 and the polypropylene fiber yarn in S2 are both preliminarily formed yarns.

8. The method for preparing high-strength nylon filament according to claim 6, characterized in that: In S4, heating is performed by hot air supply.

9. The method for preparing high-strength nylon filament according to claim 6, characterized in that: In the S6, the freezing spinning technology is used to perform low temperature cold drawing.

10. The method for preparing high-strength nylon filament according to claim 6, characterized in that: In the S7, ethanol is used for sealing and cleaning, and the mixture is dried in a sealed container.

Citation Information

Patent Citations

  • Fluffy polyamide filament and preparation method thereof

    CN117144528A

  • High-elasticity air coated yarn

    CN211848270U

  • Covered yarn

    JP2003278043A

  • Method for manufacturing an elastic yarn by melt spinning extrusion

    TW202413754A