Negative pole piece as well as preparation method and application thereof
By setting a first film layer with high surface energy and a second film layer with low surface energy on the current collector, the problems of lithium dendrites and side reactions in negative electrode-free lithium metal batteries are solved, achieving uniform lithium deposition and improved battery performance.
Patent Information
- Application Number
- CN202411174433.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-05
AI Technical Summary
Negative electrode-free lithium metal batteries suffer from lithium dendrite formation and dead lithium problems during charging and discharging, and the side reactions between lithium metal and electrolyte are severe, hindering their commercial application.
A first film layer and a second film layer are sequentially disposed on the current collector. The first film layer is composed of a first polymer with high surface energy, and the second film layer is composed of a second polymer with low surface energy. The first film layer improves lithium affinity, and the second film layer serves as a passivation layer to block the reaction between lithium metal and electrolyte.
It effectively suppresses the formation of lithium dendrites, improves the uniform deposition of lithium metal, reduces side reactions between lithium metal and electrolyte, and enhances the coulombic efficiency and cycle performance of the battery.
Smart Images

Figure BDA0005010322180000121 
Figure BDA0005010322180000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a negative electrode sheet and a preparation method and application thereof. Background Art
[0002] The advent of the global electric energy era has promoted the vigorous development of the comprehensive electrification of air and ground transportation, and at the same time has put forward higher and higher requirements for power batteries. At present, traditional lithium-ion batteries have approached the energy density limit and are difficult to meet the requirements of a wide range of application scenarios. Because the metal lithium negative electrode has the lowest reduction potential (-3.04V) and extremely high theoretical specific capacity (3860mAh / g), it is considered to be the most promising negative electrode material for the next generation of lithium batteries. However, lithium metal batteries generally have problems such as lithium dendrites, "dead lithium" and huge volume expansion during the charge and discharge cycle, which seriously hinders the commercial application of lithium metal batteries.
[0003] Anode-free lithium metal batteries are an innovative battery technology that can maximize the energy density of batteries by removing traditional active cathode materials or lithium metal such as graphite, silicon, and phosphorus. However, the copper current collector of the conventional anode is non-lithium-philic and easily forms lithium dendrites and dead lithium during the electrodeposition-stripping process, which damages battery performance and safety, and seriously hinders the commercial application of cathode-free lithium metal batteries. In order to solve the defects of the above-mentioned cathode-free lithium metal batteries, a series of improvements have been made in the existing technology.
[0004] For example, CN115832213A discloses a lithium-free negative electrode plate with a lithium-philic coating, wherein the negative electrode plate includes a current collector and a lithium-free negative electrode film layer, the lithium-free negative electrode film layer is coated on the surface of the current collector, and the lithium-free negative electrode film layer contains a first negative electrode active material, the first negative electrode active material includes a hollow hollow carbon material and a lithium-philic substance, and the lithium-philic substance is not loaded with lithium metal, and the lithium-philic substance is loaded on the inner surface of the hollow carbon material. The lithium-philic coating used in the prior art can reduce the deposition overpotential of lithium metal on the negative electrode plate and effectively inhibit the formation of lithium dendrites. However, although the lithium-philic coating is an effective strategy to inhibit lithium dendrites, due to the lack of an effective passivation protective layer, the deposited lithium metal will still have serious side reactions with the electrolyte.
[0005] Another example is CN112771693A, which discloses a three-dimensional composite metal lithium negative electrode, wherein the composite metal lithium negative electrode includes metal lithium particles and a three-dimensional polymer skeleton, the metal lithium particles are filled in the three-dimensional polymer skeleton, and the three-dimensional polymer skeleton includes a lithium-philic fragment, an active site, and a polymer-containing portion. This prior art can alleviate the volume expansion during electrodeposition or stripping by using a lithium-philic three-dimensional carbon skeleton composite negative electrode, and can inhibit the side reaction of metal lithium with the electrolyte. However, a larger specific surface area of the metal lithium negative electrode will cause more serious electrolyte side reactions.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The first purpose of the present invention is to provide a negative electrode plate suitable for a negative electrode-free lithium metal secondary battery; it is mainly used to solve the technical problem of being unable to take into account the side reactions between the negative electrode and the electrolyte when solving electrochemical and safety defects such as lithium dendrites or dead lithium in the field of negative electrode-free batteries.
[0008] The second object of the present invention is to provide a method for preparing the negative electrode plate, which has the advantages of being simple and easy to operate, having low equipment requirements, and having strong stability in the output electrode plates, and can meet the needs of mass production.
[0009] The third object of the present invention is to provide a secondary battery having the electrochemical performance advantages introduced by the negative electrode plate.
[0010] A fourth object of the present invention is to provide an electrical device.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] A negative electrode plate comprises a current collector, and a first film layer and a second film layer sequentially arranged on the current collector;
[0013] The first film layer comprises a first polymer, and the second film layer comprises a second polymer;
[0014] The surface energy of the first polymer is ≥40 mJ / m 2 , the surface energy of the second polymer is ≤30mJ / m 2 .
[0015] A method for preparing the negative electrode sheet comprises the following steps:
[0016] A first solution and a second solution including a first polymer and a second polymer are independently prepared; the first solution is applied to the surface of a current collector, and a current collector loaded with a first film layer is obtained after a first heat treatment; the second solution is applied to the surface of the first film layer, and a negative electrode plate is obtained after a second heat treatment.
[0017] A secondary battery comprises the negative electrode plate.
[0018] An electrical device comprises the secondary battery.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention provides a negative electrode plate, which is formed by sequentially arranging a first film layer and a second film layer on a current collector, wherein a first polymer contained in the first film layer has a higher surface energy and a high affinity for lithium, and correspondingly, a second polymer contained in the second film layer has a lower surface energy and a low affinity for lithium; during the charging process, lithium metal will be deposited between the first film layer and the second film layer; the high lithium affinity of the first film layer can reduce the nucleation potential of lithium metal deposition, which is beneficial to the uniform deposition of lithium metal and effectively inhibits the formation of lithium dendrites.
[0021] At the same time, the high surface energy of the first polymer in the first film layer is also more conducive to forming strong adhesion on the surface of the current collector; on the contrary, the surface energy difference between the second film layer and lithium is large, and the interface energy between the two is high, which makes lithium tend to form large-sized particles when deposited, further inhibiting the formation of lithium dendrites. In addition, the second film layer acts as a passivation layer to block the side reactions between the deposited lithium metal and the electrolyte, reduce the consumption of active lithium, and improve the coulombic efficiency.
[0022] Therefore, the present invention significantly improves the performance of a lithium battery comprising the negative electrode plate by limiting the structure and composition properties of the negative electrode plate; it has many electrochemical performance advantages such as reducing the nucleation potential of lithium metal, inhibiting the growth of lithium dendrites, increasing the battery current density, and reducing the side reactions between the negative electrode and the electrolyte, thereby achieving the effect of improving the coulombic efficiency and cycle performance of the battery. DETAILED DESCRIPTION
[0023] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the terms "first", "second" and "third" are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.
[0024] The first aspect of the present invention is to provide a negative electrode plate. The negative electrode plate comprises a current collector, and a first film layer and a second film layer sequentially arranged on the current collector; wherein the first film layer comprises a first polymer, and the second film layer comprises a second polymer; and the surface energy of the first polymer is ≥40mJ / m 2 , the surface energy of the second polymer is ≤30mJ / m 2 .
[0025] As a preferred embodiment, the first film layer and the second film layer are arranged on one side or both sides of the current collector; that is, the negative electrode plate described in the present invention can be a structure of "second film layer-first film layer-current collector-first film layer-second film layer", or a structure of "current collector-first film layer-second film layer".
[0026] As a preferred embodiment, the surface energy of the first polymer is 40 to 60 mJ / m 2 The surface energy of the second polymer is 10 to 30 mJ / m 2 In some optional embodiments, the surface energy of the first polymer includes but is not limited to 40, 42, 45, 48, 50, 52, 55, 58, 60 (mJ / m 2 ), the surface energy of the second polymer includes but is not limited to 10, 12, 15, 18, 20, 22, 25, 28, 30 (mJ / m 2 ) or any two of them.
[0027] As a preferred embodiment, the surface energy is determined by a contact angle method; those skilled in the art can obtain the surface energy parameters of the polymer by using a contact angle measuring instrument and its associated analysis software.
[0028] As a preferred embodiment, the first polymer includes at least one of polymethyl methacrylate, polycarbonate, polycaprolactam, polyethylene terephthalate, polyethylene oxide, polyphenylene ether, polyhexamethylene adipamide or hydroxypropyl methylcellulose.
[0029] As a preferred embodiment, the second polymer includes at least one of polyvinylidene fluoride-hexafluoropropylene, polydimethylsiloxane, polyvinylidene fluoride, polytetrafluoroethylene or polytrifluoroethylene.
[0030] As a preferred embodiment, the current collector includes any one of copper foil, carbon-coated copper foil or composite copper foil.
[0031] As a preferred embodiment, the thickness of the first film layer is 2 μm to 7 μm, including but not limited to any one of 2, 3, 4, 5, 6, and 7 (μm) or a numerical range consisting of any two of them.
[0032] As a preferred embodiment, the thickness of the second film layer is 0.5 μm to 3 μm, including but not limited to any one of 0.5, 1, 1.5, 2, 2.5, 3 (μm) or a numerical range consisting of any two of them.
[0033] It is worth noting that the negative electrode plate of the present invention is applied to a negative electrode-free lithium metal battery, which also means that the negative electrode plate of the present invention does not contain any negative electrode active components, such as conventional natural graphite, artificial graphite, soft carbon, hard carbon, etc., or other unconventional track materials, titanium-based materials, metals or alloy materials, etc. However, in some optional embodiments of the present invention, the following components can still be designed to be added in the two film layers.
[0034] As a preferred embodiment, the first film layer further includes lithium-philic nanoparticles; the lithium-philic nanoparticles include at least one of silver oxide, zinc oxide or indium oxide.
[0035] As a more preferred embodiment, the mass ratio of the lithium-philic nanoparticles to the first polymer is (5-15):100, including but not limited to any one of 5:100, 6:100, 8:100, 10:100, 12:100, 15:100 or a numerical range consisting of any two of them.
[0036] As a more preferred embodiment, the D50 of the lithium-philic nanoparticles is 20 nm to 100 nm; in a further preferred embodiment, the D50 of the lithium-philic nanoparticles is 50 nm.
[0037] As a preferred embodiment, the first film layer further includes a conductive agent; the conductive agent includes but is not limited to at least one of carbon nanotubes, conductive carbon black or graphene.
[0038] As a more preferred embodiment, the mass ratio of the conductive agent to the first polymer is (0.5-5):100, including but not limited to any one of 0.5:100, 1:100, 2:100, 3:100, 4:100, 5:100 or a numerical range consisting of any two of them.
[0039] As a preferred embodiment, the second film layer also includes a fluorine-containing lithium salt; the fluorine-containing lithium salt includes at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF6) or lithium difluorooxalatoborate (LiDFOB).
[0040] As a more preferred embodiment, the mass ratio of the fluorine-containing lithium salt to the second polymer is (20-50):100, including but not limited to any one of 20:100, 25:100, 30:100, 35:100, 40:100, 45:100, 50:100 or a numerical range consisting of any two of them.
[0041] The second aspect of the present invention is to provide a method for preparing the negative electrode sheet. The method mainly comprises the following steps (1) to (3).
[0042] (1) A first solution and a second solution including a first polymer and a second polymer are independently prepared.
[0043] As a preferred embodiment, the solvent of the first solution includes at least one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.
[0044] As a preferred embodiment, the mass ratio of the solute to the solvent in the first solution is (0.8-1.2):1; in some more preferred embodiments, the solute and the solvent in the first solution are prepared in a 1:1 ratio.
[0045] As a preferred embodiment, the solvent of the second solution includes at least one of ethylene glycol dimethyl ether, acetonitrile, succinonitrile, dioxolane or tetrahydrofuran.
[0046] As a preferred embodiment, the mass ratio of the solute to the solvent in the second solution is (0.3-0.7):1; in some more preferred embodiments, the solute to the solvent in the second solution is prepared in a ratio of 0.5:1.
[0047] As a preferred embodiment, the preparation process of the first solution and the second solution includes auxiliary means such as stirring, oscillation, ultrasound, centrifugation, heat treatment, etc. to achieve sufficient mixing of the solvent and the solute components.
[0048] As a more preferred embodiment, in the preparation of the first solution, the mixing temperature is 20°C to 50°C, and the mixing time is 1h to 6h; in a further preferred embodiment, the mixing temperature is 30°C, and the mixing time is 3h.
[0049] As a more preferred embodiment, in the preparation of the second solution, the mixing temperature is 20°C to 50°C, and the mixing time is 1h to 4h; in a further preferred embodiment, the mixing temperature is 30°C, and the mixing time is 2h.
[0050] (2) The first solution is coated on the surface of the current collector, and after a first heat treatment, a current collector loaded with the first film layer is obtained.
[0051] (3) The second solution is applied to the surface of the first film layer, and a negative electrode plate is obtained after a second heat treatment.
[0052] As a preferred embodiment, the coating method includes but is not limited to extrusion coating, roller coating, blade coating and the like.
[0053] As a preferred embodiment, the temperature of the first heat treatment is 80°C to 120°C, and the time of the first heat treatment is 4h to 8h; in some optional embodiments, the temperature of the first heat treatment includes but is not limited to any one of 80, 85, 90, 95, 100, 105, 110, 115, 120 (°C) or a numerical range composed of any two of them, and the time of the first heat treatment includes but is not limited to any one of 4, 5, 6, 7, 8 (h) or a numerical range composed of any two of them.
[0054] As a preferred embodiment, the temperature of the second heat treatment is 40°C to 60°C, and the time of the second heat treatment is 1h to 5h; in some optional embodiments, the temperature of the second heat treatment includes but is not limited to any one of 40, 45, 50, 55, 60 (°C) or a numerical range composed of any two of them, and the time of the second heat treatment includes but is not limited to any one of 1, 2, 3, 4, 5 (h) or a numerical range composed of any two of them.
[0055] The third aspect of the present invention is to provide a secondary battery, specifically a negative electrode-free lithium metal battery. The secondary battery includes the negative electrode plate. It is understandable that, in addition to the negative electrode plate described in the first aspect of the present invention, the secondary battery should include a positive electrode plate, an electrolyte, a diaphragm, etc., as well as other necessary or non-essential functional elements or packaging components, etc., and those skilled in the art can make any selection and combination thereof; when the negative electrode plate described in the present invention is included in the secondary battery, any other functional elements present in the secondary battery can be regarded as an embodiment of the present invention.
[0056] The fourth aspect of the present invention is to provide an electric device. The electric device includes the secondary battery. The electric device can be any device or apparatus that relies on electric energy to work or operate, including but not limited to new energy vehicles, building electrical equipment, industrial electrical appliances, household and agricultural electrical appliances, etc.; when including the secondary battery, any electric device equipped with the secondary battery can belong to an embodiment of the present invention.
[0057] Example 1
[0058] S1, 10g polycarbonate (molecular weight 50000, surface energy 46mJ / m 2 ), 1 g of nano-silver oxide (D50=50 nm) and 0.2 g of carbon nanotubes were dispersed in 11 mL of dimethyl sulfoxide and stirred at 30° C. for 3 h to obtain a mixed solution I.
[0059] S2, 10g polyvinylidene fluoride-hexafluoropropylene (molecular weight 500000, surface energy 23mJ / m 2 ) and 3 g of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) were dispersed in 26 mL of ethylene glycol dimethyl ether and stirred at 30°C for 2 h to obtain a mixed solution II.
[0060] S3. Use a scraper with a scraper gap of 5 μm to evenly coat the mixed solution I on one side of the copper foil, and dry it at 100° C. for 6 hours to obtain a first film layer with a thickness of 4 μm.
[0061] S4. Use a scraper with a scraper gap of 3 μm to evenly coat the mixed solution II on the surface of the first film layer on the copper foil in S3, and dry at 50° C. for 3 hours to obtain a second film layer with a thickness of 2 μm.
[0062] Example 2
[0063] It is basically the same as Example 1, except that:
[0064] The polyacrylic acid in step S1 was replaced with branched polyethylene oxide (molecular weight 50000, surface energy 50mJ / m 2 ).
[0065] Example 3
[0066] It is basically the same as Example 1, except that:
[0067] The polyacrylic acid in step S1 was replaced with polymethyl methacrylate (molecular weight 50000, surface energy 41mJ / m 2 ).
[0068] Example 4
[0069] It is basically the same as Example 1, except that:
[0070] The polyvinylidene fluoride-hexafluoropropylene in step S2 was replaced with polyvinylidene fluoride (molecular weight 500000, surface energy 25mJ / m 2 ).
[0071] Example 5
[0072] It is basically the same as Example 1, except that:
[0073] The polyvinylidene fluoride-hexafluoropropylene in step S2 was replaced with polydimethylsiloxane (molecular weight 115000, surface energy 21mJ / m 2 ).
[0074] Example 6
[0075] It is basically the same as Example 1, except that:
[0076] In step S1, the addition of nano silver oxide is eliminated.
[0077] Example 7
[0078] It is basically the same as Example 1, except that:
[0079] In step S3, the first film layer is obtained after drying at 120° C. for 4 hours, and in step S4, the second film layer is obtained after drying at 60° C. for 1 hour.
[0080] Example 8
[0081] It is basically the same as Example 1, except that:
[0082] In step S3, the first film layer is obtained after drying at 80° C. for 8 hours, and in step S4, the second film layer is obtained after drying at 40° C. for 5 hours.
[0083] Example 9
[0084] It is basically the same as Example 1, except that:
[0085] The thickness of the first film layer in step S3 is 2 μm, and the thickness of the second film layer in step S4 is 3 μm.
[0086] Example 10
[0087] It is basically the same as Example 1, except that:
[0088] The thickness of the first film layer in step S3 is 7 μm, and the thickness of the second film layer in step S4 is 0.5 μm.
[0089] Comparative Example 1
[0090] S1, 10g polycarbonate (molecular weight 50000, surface energy 46mJ / m 2 ), 1 g of nano-silver oxide (D50=50 nm) and 0.2 g of carbon nanotubes were dispersed in 11 mL of dimethyl sulfoxide and stirred at 30° C. for 3 h to obtain a mixed solution I.
[0091] S2. Use a scraper with a scraper gap of 5 μm to evenly coat the mixed solution I on one side of the copper foil, and dry it at 100° C. for 6 hours to obtain a film layer with a thickness of 4 μm.
[0092] Comparative Example 2
[0093] S1, 10g polyvinylidene fluoride-hexafluoropropylene (molecular weight 500000, surface energy 23mJ / m 2) and 3 g of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) were dispersed in 26 mL of ethylene glycol dimethyl ether and stirred at 30°C for 2 h to obtain a mixed solution II.
[0094] S2. Use a scraper with a scraper gap of 3 μm to evenly coat the mixed solution II on the surface of the first film layer on the copper foil in S3, and dry at 50° C. for 3 hours to obtain a second film layer with a thickness of 2 μm.
[0095] Comparative Example 3: The copper foil of Example 1 was used as the negative electrode (without coating).
[0096] Test example
[0097] by As a diaphragm, the electrolyte is 1.2M LiFSI dissolved in a mixed solution of DME and TTE (the volume ratio of the two is 1:1), the negative electrode plate provided in each embodiment and comparative example is used as the working electrode, and the lithium sheet is used as the counter electrode to assemble a 2025 button battery, and the corresponding test button batteries corresponding to each embodiment and comparative example are obtained.
[0098] The specific test method is as follows:
[0099] (1) At 0.5 mA / cm 2 10 mAh of lithium was deposited onto the negative electrode at a current density of , then charged to 1 V and stripped, and the deposition overpotential was recorded;
[0100] (2) Based on step (1), continue to 2 The current density is 10 mAh to deposit lithium to the negative electrode;
[0101] (3) First, 0.5 mA / cm 2 The current density was 0.5 mA / cm 2 2 mAh of lithium was deposited at a current density of , and this step was repeated 100 times;
[0102] (4) After step (3) is completed, the 2 The battery is charged to 1V with a current density of 1V and the capacity of the battery is recorded as Q s , calculate the average coulombic efficiency = (200 + Q s ) / (200+10)*100%.
[0103] The test results are recorded in the following Table 1.
[0104] Table 1
[0105]
[0106]
[0107] As can be seen from Table 1, the button cells corresponding to each embodiment all show lower lithium deposition overpotential and higher average coulombic efficiency. Further analysis of the differences in data performance between each comparative example and each embodiment of the present invention shows that, specifically, when only a single first film layer is applied to the copper foil current collector of comparative example 1, only the lithium deposition overpotential can be reduced, but due to the lack of a passivation protective layer, there is still a more serious electrolyte side reaction, resulting in a low coulombic efficiency. When only a single second film layer is applied to the copper foil current collector of comparative example 2, the second film layer as a passivation protective layer can inhibit the side reaction between lithium metal and the electrolyte to a certain extent, but due to the poor lithium affinity of the copper foil itself, the lithium deposition overpotential is high, which easily induces the formation of lithium dendrites, resulting in a low coulombic efficiency. The bare copper foil of comparative example 3 is not conducive to uniform lithium deposition, and lacks an effective passivation protective layer, resulting in the worst coulombic efficiency. It can be seen from this that the battery using the negative electrode plate provided by the present invention can effectively induce uniform lithium deposition, inhibit the formation of lithium dendrites, and reduce the side reaction between lithium metal and the electrolyte.
[0108] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A negative electrode plate, characterized in that: The negative electrode plate comprises a current collector, and a first film layer and a second film layer sequentially arranged on the current collector; The first film layer comprises a first polymer, and the second film layer comprises a second polymer; The surface energy of the first polymer is ≥40 mJ / m 2 , the surface energy of the second polymer is ≤30mJ / m 2 .
2. The negative electrode sheet according to claim 1, characterized in that: The thickness of the first film layer is 2 μm to 7 μm; And / or, the thickness of the second film layer is 0.5 μm to 3 μm.
3. The negative electrode sheet according to claim 1, characterized in that: The first polymer comprises at least one of polymethyl methacrylate, polycarbonate, polycaprolactam, polyethylene terephthalate, polyethylene oxide, polyphenylene ether, polyhexamethylene adipamide or hydroxypropyl methylcellulose; And / or, the second polymer includes at least one of polyvinylidene fluoride-hexafluoropropylene, polydimethylsiloxane, polyvinylidene fluoride, polytetrafluoroethylene or polytrifluoroethylene.
4. The negative electrode sheet according to claim 1, characterized in that: The first film layer further comprises lithium-philic nanoparticles; the lithium-philic nanoparticles comprise at least one of silver oxide, zinc oxide or indium oxide; And / or, the first film layer further includes a conductive agent; the conductive agent includes at least one of carbon nanotubes, conductive carbon black or graphene.
5. The negative electrode sheet according to claim 1, characterized in that: The second film layer further includes a fluorine-containing lithium salt; the fluorine-containing lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate or lithium difluorooxalatoborate.
6. The method for preparing a negative electrode sheet according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: Independently preparing a first solution and a second solution including a first polymer and a second polymer; applying the first solution to the surface of a current collector, and obtaining a current collector loaded with a first film layer after a first heat treatment; The second solution is coated onto the surface of the first film layer, and a negative electrode plate is obtained after a second heat treatment.
7. The method for preparing a negative electrode sheet according to claim 6, characterized in that: The solvent of the first solution includes at least one of dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone; And / or, the solvent of the second solution includes at least one of ethylene glycol dimethyl ether, acetonitrile, succinonitrile, dioxolane or tetrahydrofuran.
8. The method for preparing a negative electrode sheet according to claim 6, characterized in that: The temperature of the first heat treatment is 80°C to 120°C, and the time of the first heat treatment is 4h to 8h; And / or, the temperature of the second heat treatment is 40° C. to 60° C., and the time of the second heat treatment is 1 hour to 5 hours.
9. A secondary battery, characterized in that: The secondary battery comprises the negative electrode sheet as claimed in any one of claims 1 to 5.
10. An electrical device, characterized in that: The electric device comprises the secondary battery as claimed in claim 9.
Citation Information
Cited By
Composite current collector and preparation method and application thereof
CN119230844A