High-entropy solid electrolyte, preparation method thereof and lithium ion battery

By using high-entropy solid electrolytes in lithium-ion batteries, combining lithium salts, lithium-conducting polymer monomers and plasticizers, the problem of low conductivity of solid electrolytes is solved, and higher ionic conductivity and battery performance are achieved.

CN118899528APending Publication Date: 2024-11-05HONG KONG QUANTUM AI LAB LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411175086.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The low ionic conductivity of solid electrolytes limits their application potential in high energy density and high power density battery systems.

Method used

High entropy solid electrolytes, including lithium salts, lithium conduction polymer monomers and plasticizers, are used, and the sum of the components is greater than or equal to 6. By mixing and drying, a complex disordered structure is formed to optimize the migration path of ions. Improve the ionic conductivity of the electrolyte.

Benefits of technology

The ionic conductivity of lithium-ion electrolyte is significantly improved, the performance of the battery is optimized, the complexity and entropy of the electrolyte are enhanced, and the overall performance of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899528A_ABST
    Figure CN118899528A_ABST
Patent Text Reader

Abstract

The invention discloses a high-entropy solid electrolyte, a preparation method thereof and a lithium ion battery, and belongs to the technical field of lithium ion batteries. The high-entropy solid electrolyte comprises a lithium salt, a lithium-conducting polymer monomer and a plasticizer, and the sum of the types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is larger than or equal to 6. The technical problem that the ionic conductivity of the solid electrolyte is low is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a high-entropy solid electrolyte and a preparation method thereof, and a lithium-ion battery. Background Art

[0002] In the current field of lithium-ion battery technology, liquid electrolytes are widely used due to their good ionic conductivity and interface compatibility. However, with the continuous improvement of battery performance requirements, especially under high-rate charge and discharge conditions, liquid electrolytes face severe challenges. Due to local overheating and concentration gradients caused by high current density, liquid electrolytes are prone to form lithium dendrites on the negative electrode surface, which not only seriously damages the safety of the battery, but may also cause battery short circuit and rapid capacity decay.

[0003] To solve this problem, researchers are committed to developing solid electrolytes as an alternative in order to fundamentally eliminate the growth of lithium dendrites. However, while solid electrolytes exhibit excellent safety, they also expose the shortcoming of relatively low lithium ion conductivity, which limits their potential for application in high energy density and high power density battery systems.

[0004] The above contents are only used to assist in understanding the technical solution of the present application and do not constitute an admission that the above contents are prior art. Summary of the invention

[0005] The main purpose of this application is to provide a high-entropy solid electrolyte and a preparation method thereof, and a lithium-ion battery, aiming to solve the technical problem of low ionic conductivity of solid electrolytes.

[0006] To achieve the above-mentioned purpose, an embodiment of the present application provides a high-entropy solid electrolyte, comprising: a lithium salt, a lithium-conducting polymer monomer and a plasticizer, wherein the sum of the number of types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is greater than or equal to 6.

[0007] In one embodiment, the lithium salt includes at least one of LiClO4, LiPF6, LiTFSI, LiBF4, LiDFOB, LiFSI and LiDMSI.

[0008] In one embodiment, the lithium-conducting polymer monomer includes at least one of diglycidyl ether, polyethylene glycol dimethacrylate, polyetheramine, polyethylene glycol, polyacrylonitrile, polyvinylidene fluoride, polyvinyl imidazole and phenolic resin.

[0009] In one embodiment, the plasticizer includes: at least one of SiO2, TiO2, Al2O3, LiAlO2, LLZO, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, ethylene glycol dimethyl ether, diethoxyethane, diethylene glycol dimethyl ether, butyrolactone, valerolactone, caprolactone, acetonitrile, succinonitrile, 2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, trimethyl phosphate and trimethyl phosphate.

[0010] In one embodiment, the high entropy solid electrolyte includes: 5-45 wt.% lithium salt, 20-90 wt.% lithium conductive polymer monomer and 1-50 wt.% plasticizer.

[0011] In one embodiment, the mass fraction of each type of lithium conductive polymer monomer satisfies Wherein, a is the mass fraction of each type of lithium-conducting polymer monomer, A is the total mass fraction of lithium-conducting polymer monomers, and X is the number of types of lithium-conducting polymer monomers;

[0012] And / or, the mass fraction of each type of lithium salt satisfies Wherein, b is the mass fraction of each type of lithium salt, B is the total mass fraction of lithium salt, and Y is the number of types of lithium salt;

[0013] And / or, the mass fraction of each type of plasticizer satisfies Wherein, c is the mass fraction of each type of plasticizer, C is the total mass fraction of plasticizer, and Z is the number of types of plasticizer.

[0014] The present application also provides a method for preparing a high entropy solid electrolyte, which is used to prepare the high entropy solid electrolyte as described above, comprising the following steps:

[0015] Mixing a lithium salt, a lithium-conducting polymer monomer and a plasticizer to obtain a mixed solution, wherein the sum of the number of types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is greater than or equal to 6;

[0016] The mixed solution is dried to obtain a high entropy solid electrolyte.

[0017] In one embodiment, the drying temperature is 80-120°C.

[0018] In one embodiment, before the step of drying the mixed solution, the method further comprises:

[0019] The mixed solution is dripped into a container to form a liquid film, wherein the thickness of the liquid film is less than or equal to 1 mm.

[0020] An embodiment of the present application also provides a lithium-ion battery, which includes the high-entropy solid electrolyte as described above.

[0021] One or more technical solutions proposed in this application have at least the following technical effects: providing a high entropy solid electrolyte, including: a lithium salt, a lithium-conducting polymer monomer and a plasticizer, wherein the sum of the number of types of lithium salts, lithium-conducting polymer monomers and plasticizers is greater than or equal to 6. In this application, by increasing the number of types of each component of the high entropy solid electrolyte, the simple ordered structure of the original single component is broken to form a more complex disordered structure, thereby achieving an entropy increase in the entire electrolyte system and forming a high entropy solid electrolyte. In addition, the high entropy solid electrolyte of the present application is a heterogeneous multiphase system, and there are a large number of complex interfaces between different types of substances, and these interfaces further increase the complexity and entropy of the system. The high entropy effect of the high entropy solid electrolyte can optimize the migration path of ions, reduce the migration barrier, and thus improve the ionic conductivity of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the structure of a high entropy solid electrolyte membrane involved in the embodiment of the present application;

[0023] Figure 2 This is a schematic flow chart of a method for preparing a high entropy solid electrolyte according to an embodiment of the present application.

[0024] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0026] Hereinafter, the embodiment of the method for recovering lithium from waste lithium iron phosphate batteries of the present application is specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the accompanying drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0027] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0028] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0029] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0030] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0031] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0032] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0033] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and understandable, the technical solution of the present application is further described below in conjunction with the accompanying drawings and embodiments. However, the present application is not limited to the listed embodiments, and should also include any other known changes within the scope of the rights claimed in the present application.

[0034] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present application. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0035] In order to better understand the technical solution of the present application, a detailed description will be given below in conjunction with the accompanying drawings and specific implementation methods.

[0036] In conventional technology, the preparation of polymer solid electrolytes usually involves mixing the polymerized polymer with lithium salt and plasticizer, and evenly dispersing them in a low-boiling point organic solvent to form a homogeneous stable solution, which is then extended and the solvent is volatilized to finally form an electrolyte film. The disadvantage of this method is that the conductivity of the formed solid polymer electrolyte film is usually low, and because the polymer usually has a large molecular chain and poor diffusivity, it has poor interface contact with the porous positive electrode material, further affecting the overall performance of the battery.

[0037] In the embodiments of the present application, considering that the lithium-conducting polymer monomer has a small molecular weight and is usually in liquid state, the lithium-conducting polymer monomer can be directly mixed with the lithium salt and the plasticizer without adding an additional organic solvent; and then further thermally induced film formation. Since the polymer monomer has good diffusivity, it can directly penetrate into the gaps of the positive electrode material and adsorb on the surface of the positive electrode particles, and then undergo in-situ initiation and curing to obtain a positive electrode material that integrates the positive electrode and the electrolyte, thereby having better interface properties.

[0038] A first aspect of an embodiment of the present application provides a high-entropy solid electrolyte, which includes: a lithium salt, a lithium-conducting polymer monomer and a plasticizer, wherein the sum of the number of types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is greater than or equal to 6.

[0039] In one feasible embodiment, lithium salt is the ion source in the solid electrolyte, providing the migration of lithium ions in the electrolyte and realizing ion transmission during the battery charging and discharging process. The polymer monomer is the main material constituting the solid electrolyte matrix, providing a carrier for the lithium salt and supporting the structure of the entire electrolyte. The lithium-conducting polymer monomer is a polymer compound monomer that can play a good role in conducting lithium ions in the electrolyte material. Plasticizers are mainly used to improve the flexibility and processing properties of solid electrolytes, making it easier to make the electrolyte into the desired shape. At the same time, plasticizers can also promote the dissolution and dispersion of lithium salts in the polymer matrix and improve the ion conductivity.

[0040] Exemplarily, the sum of the number of types of lithium salts, lithium-conducting polymer monomers and plasticizers in the high-entropy solid electrolyte is greater than or equal to 6; for example, 7, 8, 9, 1, 0, 11, 12, 13, etc.

[0041] Exemplarily, the number of types of lithium salts is greater than or equal to 2; for example, 3, 4, 5, 6, 7, 8, etc.

[0042] Exemplarily, the number of types of lithium salts is greater than or equal to 5.

[0043] Exemplarily, the number of types of lithium-conducting polymer monomers is greater than or equal to 2; for example, 3, 4, 5, 6, 7, 8, etc.

[0044] Exemplarily, the number of types of lithium-conducting polymer monomers is greater than or equal to 5.

[0045] Exemplarily, the number of types of plasticizers is greater than or equal to 2; for example, 3, 4, 5, 6, 7, 8, etc.

[0046] Exemplarily, the number of types of plasticizers is greater than or equal to five.

[0047] In one possible embodiment, the lithium salt includes at least one of LiClO4, LiPF6, LiTFSI, LiBF4, LiDFOB, LiFSI and LiDMSI.

[0048] In one feasible embodiment, the lithium-conducting polymer monomer includes at least one of diglycidyl ether, polyethylene glycol dimethacrylate, polyetheramine, polyethylene glycol, polyacrylonitrile, polyvinylidene fluoride, polyvinyl imidazole and phenolic resin.

[0049] In one feasible embodiment, the plasticizer includes: an inorganic plasticizer and / or an organic plasticizer.

[0050] Exemplarily, the inorganic plasticizer includes at least one of SiO2, TiO2, Al2O3, LiAlO2 and LLZO.

[0051] Exemplarily, the organic plasticizer includes at least one of dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, ethylene glycol dimethyl ether, diethoxyethane, diethylene glycol dimethyl ether, butyrolactone, valerolactone, caprolactone, acetonitrile, succinonitrile, 2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, trimethyl phosphate and trimethyl phosphate.

[0052] In a feasible embodiment, the plasticizer includes: at least one of SiO2, TiO2, Al2O3, LiAlO2, LLZO, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, ethylene glycol dimethyl ether, diethoxyethane, diethylene glycol dimethyl ether, butyrolactone, valerolactone, caprolactone, acetonitrile, succinonitrile, 2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, trimethyl phosphate and trimethyl phosphate.

[0053] In one feasible embodiment, the high entropy solid electrolyte includes: 5 to 45 wt.% lithium salt, 20 to 90 wt.% lithium-conductive polymer monomer and 1 to 50 wt.% plasticizer.

[0054] Illustratively, the lithium salt is 5 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, 30 wt.%, 35 wt.%, 40 wt.%, 45 wt.%, etc.

[0055] Excessive lithium salt content may cause changes in the structure of the solid electrolyte membrane, which may cause it to lose its original stability and compactness, thereby increasing the internal resistance and leakage current of the battery, and may also increase the risk of thermal runaway of the battery during charging and discharging, reducing the safety of the battery. Lithium salt is the main source of lithium ions in the solid electrolyte. Insufficient content will lead to insufficient lithium ion supply during the charging and discharging process of the battery, thereby reducing the capacity of the battery. Therefore, the embodiment of the present application determines that the high entropy solid electrolyte includes: 5 to 45wt.% lithium salt.

[0056] Exemplarily, the lithium-conducting polymer monomer is 20wt.%, 25wt.%, 30wt.%, 35wt.%, 40wt.%, 45wt.%, 50wt.%, 55wt.%, 60wt.%, 65wt.%, 70wt.%, 75wt.%, 80wt.%, 85wt.%, 90wt.%, etc.

[0057] The polymer monomer is an important component of the solid electrolyte matrix. Excessive content may cause the matrix to be too soft, reduce its mechanical strength, affect the overall stability of the solid electrolyte, and may also hinder the transmission of lithium ions and reduce the conductivity of the solid electrolyte. Insufficient polymer monomer content may cause the solid electrolyte to be unable to form a good membrane structure, thereby affecting its basic function as an electrolyte. Therefore, the embodiment of the present application determines that the high entropy solid electrolyte includes: 20 to 90 wt.% lithium-conducting polymer monomers.

[0058] Illustratively, the plasticizer is 1 wt.%, 5 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, 30 wt.%, 35 wt.%, 40 wt.%, 45 wt.%, 50 wt.%, etc.

[0059] Although plasticizers can improve the flexibility and processing properties of solid electrolytes, excessive content will reduce the conductivity of ions in the material, affecting the performance and life of the battery. Too little content will lead to insufficient flexibility of the solid electrolyte, which is prone to cracking or breaking during the charge and discharge process. Therefore, the embodiment of the present application determines that the high entropy solid electrolyte includes: 1 to 50 wt.% plasticizer.

[0060] In a feasible embodiment, in the high entropy solid electrolyte, the mass fraction of each type of lithium-conducting polymer monomer satisfies Wherein, a is the mass fraction of each type of lithium-conducting polymer monomer, A is the total mass fraction of lithium-conducting polymer monomers, and X is the number of types of lithium-conducting polymer monomers.

[0061] In one feasible embodiment, in the high entropy solid electrolyte, the mass fraction of each type of lithium salt satisfies Among them, b is the mass fraction of each type of lithium salt, B is the total mass fraction of lithium salts, and Y is the number of types of lithium salts.

[0062] In one feasible embodiment, in the high entropy solid electrolyte, the mass fraction of each type of plasticizer satisfies Among them, c is the mass fraction of each type of plasticizer, C is the total mass fraction of plasticizers, and Z is the number of types of plasticizers.

[0063] In this embodiment, the mass fraction of each type of lithium-conducting polymer monomer is limited to meet 0.75)%,the mass fraction of various lithium salts meets And the mass fraction of various plasticizers meets This makes the contents of each component in the solid electrolyte close, which can significantly increase the mixing entropy of the system.

[0064] In one possible implementation, referring to Figure 1The solid electrolyte 100 can be further combined with a polypropylene and / or polyethylene film 200, and the polypropylene and / or polyethylene film 200 can be used as an inactive support to obtain a high entropy solid electrolyte membrane, thereby enhancing the mechanical processing performance of the finished product.

[0065] In this embodiment, a high entropy solid electrolyte is provided, including: a lithium salt, a lithium-conducting polymer monomer and a plasticizer, wherein the sum of the number of types of lithium salts, lithium-conducting polymer monomers and plasticizers is greater than or equal to 6. In the present application, by increasing the number of types of each component of the high entropy solid electrolyte, the simple ordered structure of the original single component is broken, and a more complex disordered structure is formed, thereby achieving an entropy increase in the entire electrolyte system and forming a high entropy solid electrolyte. In addition, the high entropy solid electrolyte of the present application is a heterogeneous multiphase system, and there are a large number of complex interfaces between different types of substances, and these interfaces further increase the complexity and entropy of the system. The high entropy effect of the high entropy solid electrolyte can optimize the migration path of ions, reduce the migration barrier, and thus improve the ionic conductivity of the electrolyte.

[0066] Furthermore, the present invention also provides a method for preparing a high entropy solid electrolyte. The method for preparing a high entropy solid electrolyte comprises the following steps:

[0067] Step S10, mixing a lithium salt, a lithium-conducting polymer monomer and a plasticizer to obtain a mixed solution, wherein the sum of the number of types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is greater than or equal to 6;

[0068] In a feasible embodiment, a solid lithium salt, a liquid lithium-conducting polymer monomer and a solid plasticizer are stirred and mixed at a temperature of 20 to 50° C. to obtain a mixed solution, wherein the sum of the number of types of lithium salt, lithium-conducting polymer monomer and plasticizer is greater than or equal to 6.

[0069] For example, the stirring and mixing temperature can be 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc. If the temperature is too low, it may be difficult to mix the components evenly, and if the temperature is too high, it may induce polymerization of the lithium-conducting polymer monomer. Therefore, the stirring and mixing temperature is determined to be 20-50°C in the embodiment of the present application.

[0070] Step S20, drying the mixed solution to obtain a high entropy solid electrolyte.

[0071] In a feasible embodiment, the mixed solution is dripped into a container to form a liquid film with a thickness less than or equal to 1 mm, and the liquid film is dried at a temperature of 80 to 120° C. to achieve thermally induced film formation and obtain a high entropy solid electrolyte.

[0072] Illustratively, the drying temperature may be 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, etc.

[0073] In this embodiment, considering that the lithium-conducting polymer monomer has a small molecular weight and is usually in liquid state, the lithium-conducting polymer monomer can be directly mixed with the lithium salt and the plasticizer without adding an additional organic solvent; and then further thermally induced film formation. Since the polymer monomer has good diffusivity, it can directly penetrate into the gaps of the positive electrode material and adsorb on the surface of the positive electrode particles, and then undergo in-situ initiation and curing to obtain a positive electrode material with a positive electrode and an electrolyte integrated, thereby having better interface properties.

[0074] In order to enable the details and operations of the above embodiments of the present application to be clearly understood by those skilled in the art, and to significantly demonstrate the improved performance of the embodiments of the present application, the above technical solutions are illustrated by means of multiple embodiments below.

[0075] Example 1

[0076] Lithium-conducting polymer monomer: 1.5 g diglycidyl ether, 0.5 g polyetheramine and 1.5 g polyethylene glycol dimethacrylate;

[0077] Lithium salt: 0.4gLiTFSI and 0.4gLiFSI;

[0078] Plasticizer: 1.5g succinonitrile and 0.5g LLZO powder;

[0079] The above materials were uniformly mixed to form a stable suspension, which was then dripped onto an evaporating dish and polymerized in an oven at 95°C for 2 hours to obtain a high entropy solid electrolyte. The lithium ion conductivity was measured to be 1.2×10 -3 S / cm.

[0080] Example 2

[0081] Lithium-conducting polymer monomer: 1.5 g diglycidyl ether, 0.5 g polyetheramine, 1.5 g polyethylene glycol dimethacrylate and 1.5 g polyethylene glycol;

[0082] Lithium salt: 0.4gLiTFSI, 0.4gLiFSI and 0.2gLiClO4;

[0083] Plasticizer: 1.5 g succinonitrile, 0.5 g LLZO powder and 0.8 g ethylene carbonate;

[0084] The above materials were uniformly mixed to form a stable suspension, which was then dripped onto an evaporating dish and polymerized in an oven at 95°C for 2 hours to obtain a high entropy solid electrolyte. The lithium ion conductivity was measured to be 1.6×10 -3 S / cm.

[0085] Example 3

[0086] Lithium-conducting polymer monomer: 1.0g diglycidyl ether, 0.5g polyetheramine, 1.5g polyethylene glycol dimethacrylate, 1.5g polyethylene glycol, 0.5g polyvinylidene fluoride;

[0087] Lithium salt: 0.2g LiTFSI, 0.2g LiFSI, 0.2g LiPF6, 0.2g LiDFOB and 0.2g LiClO4;

[0088] Plasticizer: 1.0 g succinonitrile, 0.25 g LLZO powder, 0.25 g Al2O3 powder, 0.2 g 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether and 0.6 g ethylene carbonate;

[0089] The above materials were uniformly mixed to form a stable suspension, which was then dripped onto an evaporating dish and polymerized in an oven at 80°C for 4 hours to obtain a high entropy solid electrolyte. The lithium ion conductivity was measured to be 2.3×10 -3 S / cm.

[0090] Comparative Example 1

[0091] Lithium-conducting polymer monomer: 8g polyethylene oxide;

[0092] Lithium salt: 1gLiTFSI;

[0093] Plasticizer: 1g ethylene carbonate;

[0094] The above materials were dispersed in 10g acrylonitrile solution, and after being evenly dispersed, they were dripped on an evaporating dish to fully evaporate the solvent to obtain a solid electrolyte. The lithium ion conductivity was measured to be 8.5×10 -5 S / cm.

[0095] Comparative Example 2

[0096] Lithium-conducting polymer monomer: 3g polyethylene glycol dimethacrylate;

[0097] Lithium salt: 0.8gLiTFSI;

[0098] Plasticizer: 1.5g LLZO powder;

[0099] The above materials were uniformly mixed to form a stable suspension, which was then dripped onto an evaporating dish and polymerized in an oven at 95°C for 2 hours to obtain a high entropy solid electrolyte. The lithium ion conductivity was measured to be 9.2×10 -6 S / cm.

[0100] Comparative Example 3

[0101] Lithium-conducting polymer monomer: 2.4 g diglycidyl ether, 1.2 g polyetheramine;

[0102] Lithium salt: 0.4gLiTFSI and 0.4gLiFSI;

[0103] Plasticizer: 2.0g LLZO powder;

[0104] The above materials were uniformly mixed to form a stable suspension, which was then dripped onto an evaporating dish and polymerized in an oven at 95°C for 2 hours to obtain a high entropy solid electrolyte. The lithium ion conductivity was measured to be 8.6×10 -5 S / cm.

[0105] The solid electrolyte prepared in the above comparative example 1 is a conventional PEO electrolyte, and the main problem it has is that the linear structure is easy to crystallize, which greatly reduces the lithium conductivity. The polyetheramine used in Examples 1 and 2 of the present application is rich in EO groups that are easy to conduct lithium, but at the same time, through the modification of other steric hindered functional groups, the randomness of the polymer structure is greatly improved, the probability of EO group crystallization is reduced, the lithium conductivity is avoided, and the entropy value of the system is increased.

[0106] According to the experimental results of the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 3, the ionic conductivity of the solid electrolyte can be effectively improved by increasing the number of types of each component of the high-entropy solid electrolyte. Among them, when the sum of the number of types between the lithium-conducting polymer monomer and the plasticizer is increased from 5 (Comparative Example 3) to 6 (Example 1), the lithium ion conductivity is significantly improved, and as the number of component types increases, the ionic conductivity is further improved.

[0107] The above are only preferred embodiments of the present application, and do not limit the scope of the present application. For those skilled in the art, the present application may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of patent protection of the present application.

Claims

1. A high entropy solid electrolyte, characterized in that: The high entropy solid electrolyte includes: a lithium salt, a lithium-conducting polymer monomer and a plasticizer, wherein the sum of the number of types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is greater than or equal to 6.

2. The high entropy solid electrolyte according to claim 1, characterized in that The lithium salt includes at least one of LiClO4, LiPF6, LiTFSI, LiBF4, LiDFOB, LiFSI and LiDMSI.

3. The high entropy solid electrolyte according to claim 1, characterized in that The lithium-conducting polymer monomer comprises at least one of diglycidyl ether, polyethylene glycol dimethacrylate, polyetheramine, polyethylene glycol, polyacrylonitrile, polyvinylidene fluoride, polyvinyl imidazole and phenolic resin.

4. The high entropy solid electrolyte according to claim 1, characterized in that The plasticizer includes at least one of SiO2, TiO2, Al2O3, LiAlO2, LLZO, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, ethylene glycol dimethyl ether, diethoxyethane, diethylene glycol dimethyl ether, butyrolactone, valerolactone, caprolactone, acetonitrile, succinonitrile, 2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, trimethyl phosphate and trimethyl phosphate.

5. The high entropy solid electrolyte according to claim 1, characterized in that The high entropy solid electrolyte comprises: 5-45 wt.% lithium salt, 20-90 wt.% lithium conductive polymer monomer and 1-50 wt.% plasticizer.

6. The high entropy solid electrolyte according to claim 1, characterized in that The mass fraction of each type of lithium-conducting polymer monomer meets Wherein, a is the mass fraction of each type of lithium-conducting polymer monomer, A is the total mass fraction of lithium-conducting polymer monomers, and X is the number of types of lithium-conducting polymer monomers; And / or, the mass fraction of each type of lithium salt satisfies Wherein, b is the mass fraction of each type of lithium salt, B is the total mass fraction of lithium salt, and Y is the number of types of lithium salt; And / or, the mass fraction of each type of plasticizer satisfies Wherein, c is the mass fraction of each type of plasticizer, C is the total mass fraction of plasticizer, and Z is the number of types of plasticizer.

7. A method for preparing a high entropy solid electrolyte, characterized in that: For preparing a high entropy solid electrolyte as claimed in any one of claims 1 to 6, the method comprises the following steps: Mixing a lithium salt, a lithium-conducting polymer monomer and a plasticizer to obtain a mixed solution, wherein the sum of the number of types of the lithium salt, the lithium-conducting polymer monomer and the plasticizer is greater than or equal to 6; The mixed solution is dried to obtain a high entropy solid electrolyte.

8. The method according to claim 7, characterized in that The drying temperature is 80-120℃.

9. The method according to claim 7, characterized in that Before the step of drying the mixed solution, the method further comprises: The mixed solution is dripped into a container to form a liquid film, wherein the thickness of the liquid film is less than or equal to 1 mm.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the high-entropy solid electrolyte according to any one of claims 1 to 6.

Citation Information

Cited By

  • High-entropy hydroxide composite solid electrolyte and preparation method thereof

    CN120073055A

  • High-entropy hydroxide composite solid-state electrolyte and preparation method thereof