Quasi-solid-state double-layer ion thermal oxidation reduction battery with high open-circuit voltage
By using quasi-solid bilayer ion structure and graphite electrodes in thermal redox batteries, the problems of low thermal power of traditional thermoelectric materials and leakage of liquid systems are solved, high open circuit voltage and stable voltage improvement are achieved, and new ways to prepare high heat Ionic thermoelectric materials with electrical power.
Patent Information
- Application Number
- CN202410901808.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Traditional electronic thermoelectric materials and thermal redox batteries based on thermal redox effects have problems in practical applications such as low thermal power and inability to operate continuously for a long time, especially in liquid systems, where there is a risk of leakage and limited voltage increase effect.
Quasically solid double-layer ionic thermal oxidation and reduction cells are prepared by using gels containing single oxide ions and gels containing single reducing ions on the cold and hot sides, respectively, and assembled with graphite wafer electrodes. , forming a high voltage battery structure.
A stable and high open circuit voltage is achieved, which can further increase the voltage when the temperature difference is established. The material components are simple, the configuration method is easy, the preparation process is gentle, and it has universal applicability. It provides p-type and n-type ionic thermoelectric materials with high thermal power. New ways.
Smart Images

Figure CN118900615A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoelectric materials, in particular to a quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage. Background Art
[0002] Waste heat plays an important role in the energy industry. Waste heat resources are commonly found in industrial fields such as steel, chemical industry, light industry, and food production. They are utilizable heat energy released during the production process. In the process of utilizing fossil energy in the industrial sector, only 40% of the energy is effectively utilized, and the remaining 60% is eventually converted into waste heat. Therefore, new technologies need to be developed to effectively utilize available thermal energy resources for power generation. Electronic thermoelectric materials use narrow bandgap semiconductors based on the Seebeck effect, which plays an important role in converting thermal energy into useful electrical energy. However, the thermal power (S) of traditional electronic thermoelectric materials is relatively low, only tens of microvolts per Kelvin (μV K -1 ), which makes it very difficult to generate enough voltage for practical applications. In contrast, ionic thermoelectric materials exhibit huge Seebeck coefficients, reaching several millivolts per kelvin (mV K -1 ), ionic thermoelectric materials based on the Soret effect have a huge Seebeck coefficient, but have the defect of being unable to generate continuous current under a constant temperature difference (ΔT) and cannot work continuously for a long time.
[0003] Thermal redox batteries (TGCs) are another type of ionic thermoelectric materials based on the thermal redox effect. The redox couples (e.g., p-type redox couple ferrocyanide / ferrocyanide [Fe(CN)6 3– / Fe(CN)6 4– ]) Oxidation or reduction reactions occur at the hot electrode and cold electrode respectively (determined by the type of p / n type of the redox pair), thereby continuously generating current. Studies have shown that the thermal power of thermal redox batteries can be enhanced by increasing the concentration difference between the hot and cold sides of the redox pair ions. However, the research objects of the above methods are all based on liquid systems, and there is a risk of leakage in actual applications, and the voltage boost effect is limited, which is much lower than that of thermal diffusion systems.
[0004] Therefore, in view of the problems and shortcomings encountered by current thermoelectric materials, especially thermal redox batteries, in practical applications, it is of great practical significance to improve the open circuit voltage of thermal redox batteries to improve the overall performance. Summary of the invention
[0005] The object of the present invention is to provide a quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage to solve the problems raised by the above background technology.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage, comprising a quasi-solid-state double-layer ion thermal redox battery, wherein the quasi-solid-state double-layer ion thermal redox battery comprises a gel 1 containing a single oxidizing ion, a gel 2 containing a single reducing ion, a cold side electrode and a hot side electrode, wherein a high voltage is formed between the hot side electrode and the cold side electrode; if the quasi-solid-state double-layer ion thermal redox battery is of p-type, the gel 1 containing a single oxidizing ion is located on the cold side, and the gel 2 containing a single reducing ion is located on the hot side; if the quasi-solid-state double-layer ion thermal redox battery is of n-type, the gel 1 containing a single oxidizing ion is located on the hot side, and the gel 2 containing a single reducing ion is located on the cold side; the cold side electrode and the hot side electrode are both graphite disc electrodes, and are respectively bonded to the cold side gel and the hot side gel;
[0007] The preparation of the quasi-solid-state double-layer ion thermal redox battery comprises the following steps:
[0008] Step 1: Select the type and method of preparing the quasi-solid-state double-layer ion thermal redox battery;
[0009] Step 2: Preparation of quasi-solid gel containing single oxidation or reduction ion;
[0010] Step 3: Thermal redox battery assembly and high open circuit voltage detection.
[0011] Preferably, in step 1, the categories of the quasi-solid-state double-layer ion thermal redox battery include p-type thermal redox battery and n-type thermal redox battery, and the method includes a mixing method or an immersion method.
[0012] Preferably, when the hybrid method is used to prepare the P-type thermal redox battery in step S1, the specific method of step S2 is:
[0013] A1: Select a certain p-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion of a certain concentration, respectively.
[0014] A2: Select a certain gelable polymer material, add it to the solution prepared in A1, stir and dissolve it, and then pour it into a mold to solidify it in a certain environment.
[0015] A3: Demolding the single oxidation ion gel and the single reduction ion gel prepared in A2, mechanically bonding the two to assemble electrodes on both sides of the double-layer gel, and obtaining a p-type quasi-solid-state double-layer ion thermal redox battery.
[0016] Preferably, when the hybrid method is used to prepare the n-type thermal redox battery in step S1, the specific method of step S2 is:
[0017] B1: Select a certain n-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion of a certain concentration respectively.
[0018] B2: Select a certain gelable polymer material, add it to the solution prepared in B1, stir and dissolve it, and then pour it into a mold and solidify it in a certain environment.
[0019] B3: De-molding the single oxidation ion gel and the single reduction ion gel prepared in B2, mechanically bonding the two to assemble electrodes on both sides of the double-layer gel, and obtaining an n-type quasi-solid-state double-layer ion thermal redox battery.
[0020] Preferably, when the immersion method is used to prepare the p-type thermal redox battery in step S1, the specific method of step S2 is:
[0021] C1. Select a gelatinizable polymer material, add solvent, stir, heat and dissolve, then pour into a mold and solidify in a certain environment.
[0022] C2. Select a certain p-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion at a certain concentration.
[0023] C3. De-mold the blank gel prepared in 1 and immerse it in the electrolyte solution containing a single oxidation ion and a single reduction ion in 2 respectively; after a period of time, take them out and mechanically bond the two to both sides of the double-layer gel to assemble electrodes to obtain a p-type quasi-solid-state double-layer ion thermal redox battery.
[0024] Preferably, when the immersion method is used to prepare the p-type thermal redox battery in step S1, the specific method of step S2 is:
[0025] D1. Select a certain gelable polymer material, add solvent, stir, heat and dissolve, then pour it into a mold and solidify it in a certain environment.
[0026] D2. Select a certain n-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion at a certain concentration.
[0027] D3, demould the blank gel prepared in D1 and soak it in the electrolyte solution containing a single oxidation ion and a single reduction ion in D2 respectively. After a period of time, take them out and mechanically bond them to the two sides of the double-layer gel to assemble electrodes, and obtain an n-type quasi-solid-state double-layer ion thermal redox battery.
[0028] Preferably, in step B1, the temperature of the PVA solution in a water bath is 40-80° C., and it needs to be stirred for 1 hour to completely dissolve.
[0029] Preferably, in step B4, the freezing temperature of the polytetrafluoroethylene mold is -5 to -10°C and needs to be frozen for 1 hour.
[0030] Preferably, in step C6, the solution water bath temperature is 70-90°C.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The present invention adopts a mixing method or an immersion method to prepare a gel containing a single oxidation or reduction ion, and then assembles the gel and an electrode to obtain a quasi-solid-state double-layer ion thermal redox battery with a high open circuit voltage.
[0033] The present invention selects a typical redox pair, adopts a simple gel preparation and treatment method, and matches it with a graphite electrode. The constructed quasi-solid-state double-layer ion thermal redox battery has a stable and high open circuit voltage, and the voltage will be further improved when the temperature difference is established.
[0034] The material of the present invention has simple components, easy configuration, mild reaction conditions in the preparation process, simple steps, and is green and environmentally friendly. It has universal applicability and provides a new way to prepare p-type and n-type ionic thermoelectric materials with high thermoelectric power. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 A schematic diagram of the composition of a quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to the present invention;
[0036] Figure 2 A single cold side electrode or reduced ion gel prepared in Examples 2-5;
[0037] Figure 3 A schematic diagram of the operation of a double-layer thermal redox battery of a quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to the present invention;
[0038] Figure 4 The voltage variation with temperature difference of the quasi-solid-state double-layer ion thermal redox battery (DTGB) in Example 1 of the present invention and the conventional single-layer thermal redox battery (TGC) is compared;
[0039] Figure 5 The voltage maintenance time images of the quasi-solid-state double-layer ion thermal redox battery (DTGB) and the traditional single-layer thermal redox battery (TGC) in Example 1 of the present invention;
[0040] Figure 6 The high open circuit voltage data of Examples 1-4 of the quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage of the present invention are presented.
[0041] In the figure:
[0042] 1. Gel 1; 2. Gel 2; 3. Cold side electrode; 4. Hot side electrode. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the implementation regulations described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Embodiment 1
[0045] Reference Figure 1-6 As shown: a quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage, including a quasi-solid-state double-layer ion thermal redox battery, the double-layer quasi-solid-state thermal redox battery includes a gel 1 containing a single oxidizing ion, a gel 2 containing a single reducing ion, a cold side electrode 3 and a hot side electrode 4, a high voltage is formed between the hot side electrode 4 and the cold side electrode 3; if the quasi-solid-state double-layer ion thermal redox battery is of p-type, the gel 1 containing a single oxidizing ion is located on the cold side, and the gel 2 containing a single reducing ion is located on the hot side; if the quasi-solid-state double-layer ion thermal redox battery is of n-type, the gel 1 containing a single oxidizing ion is located on the hot side, and the gel 2 containing a single reducing ion is located on the cold side; the cold side electrode 3 and the hot side electrode 4 are both graphite disc electrodes, and are respectively bonded to the cold side gel and the hot side gel;
[0046] The preparation of the quasi-solid-state double-layer ion thermal redox battery includes the following steps:
[0047] Step 1: Select the type and method of preparing the quasi-solid-state double-layer ion thermal redox battery;
[0048] Step 2: Preparation of quasi-solid gel containing single oxidation or reduction ion;
[0049] Step 3: Thermal redox battery assembly and high open circuit voltage detection:
[0050] In step 1, the categories of the quasi-solid-state double-layer ion thermal redox battery include p-type thermal redox battery and n-type thermal redox battery, and the method includes a mixing method or an immersion method.
[0051] Embodiment 2
[0052] This embodiment provides a P-type thermal redox battery prepared based on a hybrid method, and the preparation method of the P-type thermal redox battery is as follows:
[0053] A1, prepare 20ml, 0.2mol L-1 Concentration of potassium ferrocyanide solution and potassium ferrocyanide solution, the solvent is ethylene glycol and deionized water, and the mass ratio of the mixed solvent is 1:5;
[0054] A2, add 3g gelatin and stir in a water bath at 40℃ for 2h, then take 1ml of the mixed solution and drop it into a polytetrafluoroethylene mold. The mold is a 4*4 array, and the diameter of each unit cylinder is 14mm;
[0055] A3. Add 2-3 drops of 0.5% glutaraldehyde solution to each unit;
[0056] A4, then placed in a refrigerator, cooled at 0-2°C for 3h, then removed from the mold, to obtain a p-type gelatin hydrogel of potassium ferrocyanide and potassium ferrocyanide ( Figure 2 a);
[0057] A5. The demolded potassium ferrocyanide hydrogel and potassium ferrocyanide hydrogel are laminated together, with the potassium ferrocyanide hydrogel serving as the hot-side working end and the potassium ferrocyanide hydrogel serving as the cold-side working end. The two are laminated together to obtain a p-type potassium ferrocyanide and potassium ferrocyanide double-layer hydrogel.
[0058] The electrodes are made of graphite disc electrodes. Due to the good viscosity of the hydrogel, it can make good contact with the electrodes. Finally, an open circuit voltage of 0.2V is achieved under a temperature difference of 0K, and the voltage will rise further when a temperature difference is applied.
[0059] Embodiment 3
[0060] This example provides an n-type thermal redox battery prepared based on a hybrid method, and the preparation method of the n-type thermal redox battery is as follows:
[0061] B1. Prepare two groups of 20g PVA solution with 15% mass fraction of dimethyl sulfoxide as solvent, then place the PVA solution in a water bath, adjust the temperature to 60°C, and stir for 1h to completely dissolve it;
[0062] B2, take 4mmol of ferric perchlorate and ferrous perchlorate respectively, add 5g of deionized water to make 0.8mol L -1 Ferric perchlorate and ferrous perchlorate solutions;
[0063] B3. Add ferric perchlorate and ferrous perchlorate solutions into the two groups of completely dissolved PVA solutions respectively, and continue stirring in a water bath for 1 hour;
[0064] B4. Take 1 ml of the mixed solution and drop it into the polytetrafluoroethylene mold, then freeze it in a refrigerator at -8°C for 1 hour. Then, place the polytetrafluoroethylene mold at room temperature until the sample thaws. Repeat the freeze-thaw process 3 times.
[0065] B5. The gel sample is removed from the mold, and the ferric perchlorate gel is used as the hot side working end, and the ferrous perchlorate gel is used as the cold side working end, and then the two are bonded together to obtain an n-type ferric perchlorate and ferrous perchlorate polyvinyl alcohol hydrogel ( Figure 2 b).
[0066] The demoulded ferric perchlorate Fe(ClO4)3 hydrogel and ferrous perchlorate Fe(ClO4)2 hydrogel were laminated together, and graphite disc electrodes were used as electrodes to achieve an open circuit voltage of 0.23V.
[0067] Embodiment 4
[0068] This example provides a p-type thermal redox battery prepared by an immersion method, and the preparation method of the p-type thermal redox battery is as follows:
[0069] C1. Stir a mixture of 3 g PVA and 17 g deionized water in a 100°C water bath for 12 h until the PVA is completely dissolved.
[0070] C2. Place the mixed solution into a prefabricated polytetrafluoroethylene mold, and place the prefabricated polytetrafluoroethylene mold into a -17°C refrigerator and freeze for 12 hours;
[0071] C3, thawing at room temperature of 25°C for 12 h, freeze-thaw three times to obtain pure PVA hydrogel;
[0072] C4. The prepared PVA hydrogel was divided into two groups. One group was placed in 0.05 mol L -1 Soak in potassium ferrocyanide solution;
[0073] C5, group A was placed in 0.05 mol L -1 Soak in potassium ferrocyanide solution;
[0074] C6. Heat the solution in a water bath to 80°C and soak for 6 hours;
[0075] C7, obtaining p-type potassium ferrocyanide polyvinyl alcohol PVA gel and potassium ferrocyanide polyvinyl alcohol PVA gel containing a single redox ion ( Figure 2 c).
[0076] By bonding the two gels together and using graphite electrodes, an open circuit voltage of 0.19V was achieved.
[0077] Embodiment 5
[0078] This example provides a p-type thermal redox battery prepared by an immersion method, and the preparation method of the p-type thermal redox battery is as follows:
[0079] D1, weigh 2.4g AAM and dissolve it in 9.6g deionized water, add 0.024g APS initiator, 1wt% AAM and 0.024g MBA crosslinker, 1wt% AAM, and stir magnetically for 1 hour to obtain a gel precursor solution;
[0080] D2, adding the prepared precursor solution dropwise into a polytetrafluoroethylene mold and initiating at 60°C for 12 hours to obtain a polyacrylamide hydrogel;
[0081] D3, soak the prepared hydrogels in 0.05M potassium ferrocyanide and 0.05M potassium ferrocyanide solutions for 12 hours, then take them out and laminate the two gels ( Figure 2 d).
[0082] Using graphite electrodes, an open circuit voltage of 0.21V was achieved.
[0083] In the present invention, a gel containing a single oxidation or reduction ion is prepared by a mixing method or an immersion method, and then the gel and the electrode are assembled to obtain a quasi-solid-state double-layer ion thermal redox battery with a high open circuit voltage. In addition, a simple gel preparation and treatment method is adopted, and a graphite electrode is used. The constructed quasi-solid-state double-layer ion thermal redox battery has a stable and high open circuit voltage, and the voltage will be further improved when the temperature difference is established. Secondly, the material components are simple, the configuration method is easy, the reaction conditions of the preparation process are mild, the steps are simple, and it is green and environmentally friendly. At the same time, it has universal applicability, and provides a new way to prepare p-type and n-type ion thermoelectric materials with high thermoelectric power.
[0084] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage, characterized in that: The invention comprises a quasi-solid-state double-layer ion thermal redox battery, wherein the quasi-solid-state double-layer ion thermal redox battery comprises a gel 1 (1) containing a single oxidizing ion, a gel 2 (2) containing a single reducing ion, a cold side electrode (3) and a hot side electrode (4), wherein a high voltage is formed between the hot side electrode (4) and the cold side electrode (3); if the quasi-solid-state double-layer ion thermal redox battery is of p-type, the gel 1 (1) containing a single oxidizing ion is located on the cold side, and the gel 2 (2) containing a single reducing ion is located on the hot side; if the quasi-solid-state double-layer ion thermal redox battery is of n-type, the gel 1 (1) containing a single oxidizing ion is located on the hot side, and the gel 2 (2) containing a single reducing ion is located on the cold side; the cold side electrode (3) and the hot side electrode (4) are both graphite disc electrodes, and are respectively bonded to the cold side gel and the hot side gel; The preparation of the quasi-solid-state double-layer ion thermal redox battery comprises the following steps: S1. Select the type and method of preparing the quasi-solid-state double-layer ion thermal redox battery; S2, preparation of quasi-solid gel containing single oxidized or reduced ions; S3. Thermal redox battery assembly and high open circuit voltage detection.
2. A quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 1, characterized in that: In step S1 , the categories of the quasi-solid-state double-layer ion thermal redox battery include a p-type thermal redox battery and an n-type thermal redox battery, and the method thereof includes a mixing method or an immersion method.
3. The quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 1, characterized in that: When the hybrid method is used in step S1 to prepare the P-type thermal redox battery, the specific method of step S2 is: A1: Select a certain p-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion of a certain concentration, respectively. A2: Select a certain gelable polymer material, add it to the solution prepared in A1, stir and dissolve it, and then pour it into a mold to solidify it in a certain environment. A3: Demolding the single oxidation ion gel and the single reduction ion gel prepared in A2, mechanically bonding the two to assemble electrodes on both sides of the double-layer gel, and obtaining a p-type quasi-solid-state double-layer ion thermal redox battery.
4. A quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to any one of claim 1, characterized in that: When the hybrid method is used in step S1 to prepare the n-type thermal redox battery, the specific method of step S2 is: B1: Select a certain n-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion of a certain concentration respectively. B2: Select a certain gelable polymer material, add it to the solution prepared in B1, stir and dissolve it, and then pour it into a mold and solidify it in a certain environment. B3: De-molding the single oxidation ion gel and the single reduction ion gel prepared in B2, mechanically bonding the two to assemble electrodes on both sides of the double-layer gel, and obtaining an n-type quasi-solid-state double-layer ion thermal redox battery.
5. The quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 3, characterized in that: When the immersion method is used in step S1 to prepare the p-type thermal redox battery, the specific method of step S2 is: C1. Select a gelatinizable polymer material, add solvent, stir, heat and dissolve, then pour into a mold and solidify in a certain environment. C2. Select a certain p-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion at a certain concentration. C3. De-mold the blank gel prepared in 1 and immerse it in the electrolyte solution containing a single oxidation ion and a single reduction ion in 2 respectively; after a period of time, take them out and mechanically bond the two to both sides of the double-layer gel to assemble electrodes to obtain a p-type quasi-solid-state double-layer ion thermal redox battery.
6. The quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 3, characterized in that: When the immersion method is used in step S1 to prepare the p-type thermal redox battery, the specific method of step S2 is: D1. Select a certain gelable polymer material, add solvent, stir, heat and dissolve, then pour it into a mold and solidify it in a certain environment. D2. Select a certain n-type thermal redox ion pair, select a solvent that can dissolve the thermal redox ion pair, and prepare electrolyte solutions containing a single oxidizing ion and a single reducing ion at a certain concentration. D3, demold the blank gel prepared in D1 and immerse it in the electrolyte solution containing a single oxidation ion and a single reduction ion in D2 respectively; after a period of time, take them out and mechanically bond the two to the two sides of the double-layer gel to assemble electrodes to obtain an n-type quasi-solid-state double-layer ion thermal redox battery.
7. The quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 4, characterized in that: In step B1, the PVA solution is placed in a water bath at a temperature of 40-80°C and stirred for 1 hour to completely dissolve it.
8. The quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 4, characterized in that: In step B4, the freezing temperature of the polytetrafluoroethylene mold is -5 to -10°C and needs to be frozen for 1 hour.
9. The quasi-solid-state double-layer ion thermal redox battery with high open circuit voltage according to claim 5, characterized in that: In step C6, the solution water bath temperature is 70-90°C.
Citation Information
Patent Citations
Stretchable ionic hydrogel with high thermopower for low-grade heat harvesting
CN113571628A
Preparation method and application of high-performance thermoelectric hydrogel based on ion conduction
CN113881068A
Stretchable ion thermoelectric device and preparation method thereof
CN115566215A
Thermo electric device
KR1020180088015A
Light-emitting polymers and polymer light-emitting diodes