Method for recovering platinum group elements
By using a capture agent in a solution containing platinum group elements and controlling the ratio of oxidized platinum group elements, the problem of low recovery efficiency of platinum group elements in the prior art is solved, and efficient recovery and re-registration of platinum group elements is achieved. The platinum group content in the material is reduced and coloring is suppressed.
Patent Information
- Application Number
- CN202380028680.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-29
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art has low efficiency in recovering platinum group elements from a solution containing platinum group elements, resulting in low reuse rate of platinum group elements.
The platinum group element is adsorbed on it by using a capture agent, and the proportion of platinum group element complexes in the oxidized state is achieved efficiently recovering platinum group elements. The specific method includes using a metal-free oxidant, complexing agent and capture agent to contact the solution containing platinum group elements at the same time, and adsorb the platinum group elements through a column filled with the capture agent to improve recovery efficiency.
The recovery and reuse rate of platinum group elements are significantly improved, the content of platinum group elements in hydrogenated nitrile rubber is reduced, the coloring problem is reduced, and the mechanical strength of the material is maintained.
Smart Images

Figure BDA0005049834620000271
Abstract
Description
Technical Field
[0001] The invention relates to a method for recovering platinum group elements from a solution containing the platinum group elements. Background Art
[0002] Nitrile rubber (acrylonitrile-butadiene copolymer rubber) has been used as a material for rubber parts for automobiles such as hoses and tubes due to its effective oil resistance, mechanical properties, and chemical resistance. In addition, hydrogenated nitrile rubber (hydrogenated acrylonitrile-butadiene copolymer rubber) obtained by hydrogenating the carbon-carbon double bonds in the polymer main chain of nitrile rubber has better heat resistance and is therefore used for rubber parts such as belts, hoses, and diaphragms.
[0003] Such hydrogenated nitrile rubber can be produced, for example, by the following manufacturing process. That is, a monomer mixture containing an α,β-ethylenically unsaturated nitrile monomer and a conjugated diene monomer is emulsion polymerized, the latex of the nitrile rubber obtained by the emulsion polymerization is coagulated and dried, and then the nitrile rubber obtained by the coagulation and drying is dissolved in a water-soluble organic solvent to obtain a water-soluble organic solvent solution of the nitrile rubber, and a platinum group element-containing catalyst is added thereto as a hydrogenation catalyst to carry out hydrogenation, thereby producing the hydrogenated nitrile rubber.
[0004] On the other hand, in the hydrogenated nitrile rubber produced by such a production method, a platinum group element catalyst is used as a hydrogenation catalyst. From the viewpoint of suppressing the coloration of the finally obtained hydrogenated nitrile rubber, research is being conducted on removing the platinum group element catalyst to reduce the content of the platinum group element catalyst contained in the hydrogenated nitrile rubber.
[0005] As a technology for recovering such a platinum group element-containing catalyst, for example, the following method is disclosed in Patent Document 1: a complexing agent is added to a reaction mixture in which a hydrogenation reaction has been carried out in the presence of a platinum group element-containing catalyst supported on a carrier, the platinum group element-containing catalyst contained in the reaction mixture and detached from the carrier is complexed, the obtained complex is supported on the carrier again, and the carrier is removed from the reaction mixture.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2004-26998. Summary of the invention
[0009] Problem that the invention aims to solve
[0010] On the other hand, since the platinum group elements contained in the platinum group element-containing catalyst are expensive, the recovery and reuse of the platinum group element has been desired in recent years. In this regard, the present inventors have conducted research and found that, in the technology of the above-mentioned Patent Document 1, although the platinum group element-containing catalyst can be removed from a solution of the platinum group element-containing catalyst at a relatively high removal rate, the amount that can be recovered as the platinum group element is small. Therefore, from the viewpoint of recovery and reuse of the platinum group element, it is desired to improve this.
[0011] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a method for recovering platinum group elements capable of recovering platinum group elements with high efficiency.
[0012] Solutions for solving problems
[0013] The present inventors have conducted intensive studies to achieve the above-mentioned purpose, and as a result, have found that by using a capture agent to adsorb platinum group elements to the capture agent, when recovering platinum group elements from a solution containing platinum group elements, the proportion of platinum group elements adsorbed in the form of oxidized platinum group element complexes in the platinum group elements adsorbed to the capture agent is made to be above a prescribed level, and the platinum group elements are adsorbed to the capture agent to recover the platinum group elements, thereby solving the above-mentioned problems and completing the present invention.
[0014] That is, according to the present invention, there is provided a method for recovering platinum group elements, which is a method for recovering platinum group elements from a solution containing platinum group elements by using a capture agent and causing the platinum group elements to be adsorbed on the capture agent.
[0015] The platinum group elements are adsorbed on the trapping agent to recover the platinum group elements in a state where the ratio of the platinum group elements adsorbed in the form of an oxidized platinum group element complex among the platinum group elements adsorbed on the trapping agent is 50 mol% or more.
[0016] In the method for recovering platinum group elements of the present invention, it is preferred that the proportion of platinum group elements adsorbed in the form of platinum group element complexes in divalent or higher oxidation states among the platinum group elements adsorbed on the capture agent is 50 mol% or more, and the platinum group elements are adsorbed on the capture agent to recover the platinum group elements.
[0017] In the method for recovering platinum group elements of the present invention, it is preferred to recover the platinum group elements in the presence of a complexing agent represented by the following general formula (1).
[0018] C n H m N p O q X r (1)
[0019] (In the above general formula (1), X is an element other than C, H, N, and O, n=1 to 13, m=1 to 18, p=0 to 4, q=0 to 4, r=0 to 4, and at least one of p and q is 1 or more).
[0020] In the method for recovering platinum group elements of the present invention, it is preferred that the complexing agent is an ammonium salt, an amine or an imine.
[0021] In the method for recovering platinum group elements of the present invention, it is preferred that the solution containing platinum group elements is a solution containing platinum group elements and a polymer.
[0022] In the method for recovering platinum group elements of the present invention, it is preferred that the solution containing platinum group elements is a solution containing hydrogenated nitrile rubber and platinum group elements derived from a platinum group element-containing catalyst.
[0023] In the method for recovering platinum group elements of the present invention, it is preferred that the recovery be initiated by adsorption of the platinum group elements contained in the solution containing the platinum group elements onto the capture agent while a metal-free oxidant, a complexing agent and a capture agent are simultaneously brought into contact with a solution containing the platinum group elements.
[0024] Furthermore, in the method for recovering platinum group elements of the present invention, it is preferred that a metal-free oxidant and a complexing agent are simultaneously contacted with a solution containing platinum group elements, and a solution containing an oxidized platinum group element complex having a ratio of 50 mol% or more is passed through a column filled with a capture agent to allow the platinum group elements to be adsorbed onto the above-mentioned capture agent.
[0025] In the method for recovering platinum group elements of the present invention, it is preferred that the metal-free oxidant is hydrogen peroxide, air or oxygen.
[0026] In the method for recovering platinum group elements of the present invention, it is preferred that the capture agent is surface-treated silica.
[0027] Effects of the Invention
[0028] According to the present invention, a method for recovering platinum group elements capable of recovering platinum group elements with high efficiency can be provided. DETAILED DESCRIPTION
[0029] The method for recovering platinum group elements of the present invention is a method for recovering platinum group elements from a solution containing platinum group elements by using a capture agent to adsorb the platinum group elements onto the capture agent.
[0030] In the above-mentioned method for recovering platinum group elements, the platinum group elements are adsorbed on the capture agent in a state where the proportion of the platinum group elements adsorbed in the form of an oxidized platinum group element complex in the platinum group elements adsorbed on the capture agent is 50 mol% or more, and the platinum group elements are recovered.
[0031] <Platinum Group Elements>
[0032] First, the platinum group elements to be recovered in the recovery method of the present invention will be described.
[0033] In the recovery method of the present invention, as the platinum group element to be recovered, any platinum group element contained in a solution containing platinum group elements can be used. As a solution containing such platinum group elements, for example, platinum group elements contained in a solution containing platinum group elements and polymers can be cited. More specifically, platinum group elements from platinum group element-containing catalysts used when hydrogenated conjugated diene rubbers such as hydrogenated nitrile rubbers are obtained by hydrogenating carbon-carbon double bonds contained in conjugated diene rubbers such as nitrile rubbers can be cited. That is, platinum group elements from platinum group element-containing catalysts contained in a solution of hydrogenated conjugated diene rubbers such as hydrogenated nitrile rubbers can be cited. As an example of the hydrogenation reaction of such conjugated diene rubbers, the hydrogenation reaction of nitrile rubber is exemplified, which is described below.
[0034] As the nitrile rubber, for example, there can be mentioned a copolymer obtained by copolymerizing a monomer mixture containing at least an α,β-ethylenically unsaturated nitrile monomer and a conjugated diene monomer. As the α,β-ethylenically unsaturated nitrile monomer, there is no particular limitation as long as it is an α,β-ethylenically unsaturated compound having a nitrile group, and examples thereof include: acrylonitrile; α-halogenated acrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitriles such as methacrylonitrile, etc. In addition, as the conjugated diene monomer, there can be mentioned a conjugated diene monomer having 4 to 6 carbon atoms such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, etc.
[0035] The content of α,β-ethylenically unsaturated nitrile monomer units in the nitrile rubber is preferably 5 to 60% by weight, more preferably 10 to 50% by weight, and further preferably 15 to 50% by weight relative to all monomer units. In addition, the content of conjugated diene monomer units (including portions hydrogenated by hydrogenation) in the nitrile rubber is preferably 40 to 95% by weight, more preferably 50 to 90% by weight, and further preferably 50 to 85% by weight relative to all monomer units.
[0036] In addition, in addition to α,β-ethylenically unsaturated nitrile monomers and conjugated diene monomers, nitrile rubber can also be copolymerized with other monomers that can be copolymerized with these monomers. Examples of such other monomers that can be copolymerized include: α,β-ethylenically unsaturated monocarboxylic acid monomers such as acrylic acid and methacrylic acid; α,β-ethylenically unsaturated polycarboxylic acid monomers; α,β-ethylenically unsaturated monocarboxylic acid ester monomers such as methyl acrylate, ethyl acrylate, and n-butyl acrylate; α,β-ethylenically unsaturated dicarboxylic acid monoester monomers such as mono-n-butyl maleate and mono-n-butyl fumarate; ethylene; α-olefin monomers, aromatic vinyl monomers; fluorine-containing vinyl monomers; copolymerizable antioxidants, etc.
[0037] The hydrogenation of acrylonitrile-butadiene rubber can be carried out using a platinum group element catalyst usually. To the latex of the acrylonitrile-butadiene rubber obtained by emulsion polymerization, the hydrogenation of acrylonitrile-butadiene rubber can directly be carried out with the latex state, or the latex of the acrylonitrile-butadiene rubber obtained by emulsion polymerization can be solidified, dried and solid acrylonitrile-butadiene rubber is obtained, the obtained acrylonitrile-butadiene rubber is dissolved in an organic solvent, carried out with the state of polymer solution. Among these, from viewpoints such as catalyst activity, preferably the obtained acrylonitrile-butadiene rubber is dissolved in a water-soluble organic solvent, carries out the hydrogenation of acrylonitrile-butadiene rubber with the state of polymer solution.
[0038] The coagulation and drying of the latex of the nitrile rubber can be carried out by a known method. It is preferred to provide a treatment step of bringing the pellets obtained by coagulation into contact with an alkaline aqueous solution, and to modify the obtained nitrile rubber in such a manner that the pH of the polymer solution measured by dissolving in tetrahydrofuran (THF) is greater than 7. The pH of the polymer solution measured by dissolving in THF and adding several wt% of water to THF is preferably in the range of 7.2 to 12, more preferably in the range of 7.5 to 11.5, and most preferably in the range of 8 to 11. By the contact treatment of the pellets with the alkaline aqueous solution, solution-based hydrogenation (hydrogenation by dissolving in an organic solvent) can be rapidly performed.
[0039] The concentration of the nitrile rubber in the polymer solution during the hydrogenation reaction is preferably 1 to 70% by weight, more preferably 1 to 40% by weight, and particularly preferably 2 to 20% by weight. Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, diethyl ketone, and methyl isopropyl ketone; tetrahydrofuran, dihydrofuran, and dihydrogen ether; Ethers such as alkanes; esters such as ethyl acetate; aldehydes such as dimethylformamide; aromatic compounds such as toluene, chlorobenzene, monochlorobenzene; halogenated aliphatic compounds, etc. Among these organic solvents, ketones are particularly preferably used, and acetone is particularly preferably used.
[0040] When the hydrogenation reaction is carried out, a platinum group element catalyst can be used as a hydrogenation catalyst. As the platinum group element catalyst, as long as it is a catalyst containing a platinum group element, i.e., ruthenium, rhodium, palladium, osmium, iridium or platinum, it is not particularly limited. From the viewpoint of catalyst activity and ease of acquisition, palladium compounds and rhodium compounds are preferred, and palladium compounds are more preferred. In addition, two or more platinum group element compounds can also be used in combination. In this case, it is also preferred to use a palladium compound as the main catalyst component.
[0041] The palladium compound used is generally a II-valent or IV-valent palladium compound, and the palladium compound is in the form of a salt or a complex salt.
[0042] Examples of the palladium compound include palladium acetate, palladium cyanide, palladium fluoride, palladium chloride, palladium bromide, palladium iodide, palladium nitrate, palladium sulfate, palladium oxide, palladium hydroxide, dichloro(cyclooctadiene)palladium, dichloro(norbornadiene)palladium, dichlorobis(triphenylphosphine)palladium, sodium tetrachloropalladate, ammonium hexachloropalladate, and potassium tetracyanopalladate.
[0043] Among these palladium compounds, palladium acetate, palladium nitrate, palladium sulfate, palladium chloride, sodium tetrachloropalladate, and ammonium hexachloropalladate are preferred, and palladium acetate, palladium nitrate, and palladium chloride are more preferred.
[0044] Examples of the rhodium compound include rhodium chloride, rhodium bromide, rhodium iodide, rhodium nitrate, rhodium sulfate, rhodium acetate, rhodium formate, rhodium propionate, rhodium butyrate, rhodium valerate, rhodium naphthenate, rhodium acetylacetonate, rhodium oxide, and rhodium trihydroxide.
[0045] As the platinum group element-containing catalyst, the above-mentioned palladium compound or rhodium compound may be used directly, or a catalyst component such as the above-mentioned palladium compound or rhodium compound may be supported on a carrier to be used as a supported catalyst.
[0046] The carrier used to form the supported catalyst may be any carrier generally used as a carrier for metal catalysts. Specifically, inorganic compounds containing carbon, silicon, aluminum, magnesium, etc. are preferred. In particular, from the viewpoint of further improving the adsorption efficiency of catalyst components such as palladium compounds and rhodium compounds, as the characteristics of the carrier, it is preferred to use an average particle size of 1 μm to 500 μm and a specific surface area of 200 to 2000 m 2 / g of carrier.
[0047] Such a carrier is appropriately selected from known catalyst carriers such as activated carbon, activated clay, talc, clay, alumina gel, silica, diatomaceous earth, synthetic zeolite, etc. As a method for loading the catalyst component on the carrier, for example, an impregnation method, a coating method, a spraying method, a precipitation method, etc. can be cited. The loading amount of the catalyst component is usually 0.5 to 80% by weight, preferably 1 to 50% by weight, and more preferably 2 to 30% by weight, based on the ratio of the catalyst component to the total amount of the catalyst and the carrier. The carrier loaded with the catalyst component can be shaped into, for example, a spherical, cylindrical, polygonal prism, honeycomb, etc., according to the type of reactor, the reaction form, etc.
[0048] In addition, when the salt of platinum group elements such as palladium compounds and rhodium compounds is not loaded on a carrier but directly used as a platinum group element catalyst, it is preferred to use a stabilizer for stabilizing these compounds. By making the stabilizer present in a medium containing platinum group element catalysts such as palladium compounds and rhodium compounds dissolved or dispersed, the nitrile rubber can be hydrogenated with a high hydrogenation rate. In addition, it can also be a complexed platinum group element catalyst.
[0049] As such stabilizers, for example, polymers of vinyl compounds having polar groups in the side chains, such as polyvinyl pyrrolidone, polyvinyl alcohol, polyvinyl acetal, and polyalkyl vinyl ethers; metal salts of polyacrylic acid, such as sodium polyacrylate and potassium polyacrylate; polyethers, such as polyethylene oxide, polypropylene oxide, and ethylene oxide-propylene oxide copolymers; cellulose derivatives, such as carboxymethyl cellulose and hydroxypropyl cellulose; natural polymers, such as gelatin and albumin, etc. Among these, polymers or polyethers of vinyl compounds having polar groups in the side chains are preferred. Among the polymers of vinyl compounds having polar groups in the side chains, polyvinyl pyrrolidone and polyalkyl vinyl ethers are preferred, and polymethyl vinyl ether is more preferred. As complexing ligands, triphenylphosphine and the like can be cited.
[0050] In the hydrogenation reaction, a reducing agent may be used in combination. Examples of the reducing agent include hydrazines such as hydrazine, hydrazine hydrate, hydrazine acetate, hydrazine sulfate salts, and hydrazine hydrochloride salts; or compounds that release hydrazine.
[0051] The temperature of the hydrogenation reaction is usually 0 to 200° C., preferably 5 to 150° C., and more preferably 10 to 100° C. By setting the temperature of the hydrogenation reaction to be within the above range, the reaction rate can be made sufficient while suppressing side reactions.
[0052] The pressure of hydrogen during the hydrogenation reaction is usually 0.1 to 20 MPa, preferably 0.1 to 15 MPa, and more preferably 0.1 to 10 MPa. The reaction time is not particularly limited, but is usually 30 minutes to 50 hours. In addition, with respect to hydrogen, it is preferred to first replace the reaction system with an inert gas such as nitrogen, then replace it with hydrogen, and then pressurize it.
[0053] When a supported catalyst is used as the platinum group element-containing catalyst, the supported catalyst may be separated by filtration, centrifugal separation or the like, thereby obtaining a water-soluble organic solvent solution of hydrogenated nitrile rubber.
[0054] <Methods for recovering platinum group elements>
[0055] Next, the method for recovering platinum group elements of the present invention will be described.
[0056] The method for recovering platinum group elements of the present invention is a method for recovering platinum group elements from a solution containing platinum group elements by using a capture agent to adsorb the platinum group elements onto the capture agent.
[0057] As the solution containing platinum group elements, for example, solutions of hydrogenated conjugated diene rubbers such as the hydrogenated nitrile rubber, etc. can be cited. When the solution containing platinum group elements is a solution of hydrogenated conjugated diene rubbers such as the hydrogenated nitrile rubber, etc., solutions containing platinum group elements from platinum group element-containing catalysts can be cited. In addition, when the solution containing platinum group elements is a solution of hydrogenated conjugated diene rubbers such as the hydrogenated nitrile rubber, etc., when a supported catalyst is used as the platinum group element-containing catalyst, the supported catalyst can be separated by filtration, centrifugal separation, etc., and the solution obtained thereby can be supplied to the method for recovering platinum group elements of the present invention, or the solution in a state where the supported catalyst remains can be supplied without separation.
[0058] Furthermore, in the method for recovering platinum group elements of the present invention, a trapping agent is used, the trapping agent is brought into contact with a solution containing platinum group elements, and platinum group elements are adsorbed on the trapping agent, thereby recovering platinum group elements. At this time, the proportion of platinum group elements adsorbed in the form of oxidized platinum group element complexes among the platinum group elements adsorbed on the trapping agent is 50% by mole or more, and the platinum group elements are adsorbed on the trapping agent to recover the platinum group elements. More specifically, the proportion of platinum group elements in the form of oxidized platinum group element complexes among the platinum group elements adsorbed on the trapping agent is 50% by mole or more, and the trapping agent adsorbed with platinum group elements in this state is separated from the solution containing platinum group elements, thereby recovering the platinum group elements. According to the present invention, by adopting such a structure, platinum group elements can be recovered with high efficiency. That is, the amount of platinum group elements captured by the trapping agent can be increased (the capture rate can be increased), thereby improving the recycling rate.
[0059] Here, in the recovery method of the present invention, a trapping agent is used and the platinum group element contained in the solution containing the platinum group element is adsorbed on the trapping agent. The inventors of the present invention have focused on the state of the platinum group element adsorbed on the trapping agent and have conducted in-depth research. Specifically, the inventors of the present invention have focused on the state of the platinum group element adsorbed on the trapping agent and have conducted in-depth research and found that the state, especially the oxidation state, of the platinum group element adsorbed on the trapping agent is not necessarily the same. Furthermore, the inventors of the present invention have found that by making the proportion of the platinum group element adsorbed in the form of an oxidized platinum group element complex in the platinum group element adsorbed on the trapping agent 50 mol% or more, and recovering the trapping agent in this state, the amount of the platinum group element captured by the trapping agent can be increased (the capture rate can be improved), thereby achieving a high recovery rate.
[0060] In the recovery method of the present invention, the platinum group elements are adsorbed on the trapping agent to recover the platinum group elements in a state where the proportion of the platinum group elements adsorbed in the form of an oxidized platinum group element complex in the platinum group elements adsorbed on the trapping agent is 50 mol% or more, and it is desirable that the platinum group elements are adsorbed on the trapping agent to recover the platinum group elements in a state where the proportion of the platinum group elements adsorbed in the form of an oxidized platinum group element complex is preferably 60 mol% or more, more preferably 65 mol% or more, and further preferably 68 mol% or more. In addition, the upper limit of the platinum group elements adsorbed in the form of an oxidized platinum group element complex is not particularly limited, but is preferably 99 mol% or less.
[0061] In addition, in the recovery method of the present invention, the platinum group elements are adsorbed on the capture agent in a state where the proportion of the platinum group elements adsorbed in the form of the platinum group element complex in the oxidized state is 50 mol% or more, and the platinum group elements are recovered. From the viewpoint of increasing the amount of the platinum group elements captured by the capture agent, it is desirable to recover the platinum group elements by adsorbing the platinum group elements on the capture agent in a state where the proportion of the platinum group elements adsorbed in the form of the platinum group element complex in a divalent or higher oxidation state is 50 mol% or more. The proportion of the platinum group elements adsorbed in the form of the platinum group element complex in a divalent or higher oxidation state is preferably 60 mol% or more, more preferably 65 mol% or more, and further preferably 68 mol% or more. In addition, the upper limit is not particularly limited, but is preferably 99 mol% or less.
[0062] The ratio of the platinum group element adsorbed in the form of a platinum group element complex in an oxidized state and the ratio of the platinum group element adsorbed in the form of a platinum group element complex in a divalent or higher oxidized state can be determined, for example, by measuring the valence ratio of the platinum group element by performing XAFS measurement as described in the Examples described below.
[0063] In addition, in the recovery method of the present invention, the trapping agent is brought into contact with the solution containing the platinum group elements, and the platinum group elements are adsorbed on the trapping agent. It is believed that the ratio of the oxidized platinum group element complex in the platinum group elements adsorbed by the trapping agent (and the ratio of the platinum group element complex in a divalent or higher oxidation state) is similar to the ratio of the oxidized platinum group element complex in the solution containing the platinum group elements (and the ratio of the platinum group element complex in a divalent or higher oxidation state). That is, the trapping agent has substantially the same trapping ability for the platinum group elements, regardless of the state of the platinum group elements, that is, whether the oxidized platinum group element complex (and the platinum group element complex in a divalent or higher oxidation state) is formed, so it is believed that the above ratio of the platinum group elements adsorbed by the trapping agent is similar to the above ratio in the solution containing the platinum group elements. Therefore, in the recovery method of the present invention, it is preferred to set the ratio of the oxidized platinum group element complex in the platinum group elements contained in the solution containing the platinum group elements (and the ratio of the platinum group element complex in a divalent or higher oxidation state) to a state increased to the above range, so that it is adsorbed on the trapping agent.
[0064] In the recovery method of the present invention, examples of platinum group elements include ruthenium, rhodium, palladium, osmium, iridium, and platinum. Among these, palladium and rhodium are preferred, and palladium is more preferred.
[0065] In the recovery method of the present invention, the platinum group elements are adsorbed on the trapping agent in a state where the proportion of the platinum group elements adsorbed in the form of an oxidized platinum group element complex in the platinum group elements adsorbed on the trapping agent is 50 mol% or more, and the platinum group elements are recovered. The specific method is not particularly limited, and the following methods are preferred: a method in which a metal-free oxidant, a complexing agent and a trapping agent are simultaneously contacted with a solution containing the platinum group elements, and the recovery is started by the platinum group elements contained in the solution containing the platinum group elements being adsorbed onto the trapping agent; and a method in which a metal-free oxidant and a complexing agent are simultaneously contacted with a solution containing the platinum group elements, and then the trapping agent is contacted with the solution, and the recovery is started by the platinum group elements contained in the solution containing the platinum group elements being adsorbed onto the trapping agent.
[0066] More specifically, it is preferred that a metal-free oxidant and a complexing agent and / or a scavenger coexist in a solution containing platinum group elements, and the reaction solution in this state is heated to preferably 35 to 150° C., more preferably 40 to 140° C., thereby starting to recover the platinum group elements contained in the solution containing platinum group elements. That is, it is preferred to start the recovery of platinum group elements in a state where a metal-free oxidant and a complexing agent coexist (that is, the temperature is raised to the above temperature, thereby starting the recovery). In addition, at this time, from the viewpoint of being able to further enhance the effect of the present invention, it is more preferred that a scavenger coexists in addition to a metal-free oxidant and a complexing agent, and the solution in this state is heated to the above temperature, thereby starting to recover the platinum group elements contained in the solution containing platinum group elements.
[0067] By starting the recovery treatment of the platinum group elements in the presence of a metal-free oxidant, a complexing agent and / or a scavenger, the oxidation reaction of the platinum group elements contained in the solution containing the platinum group elements can be more appropriately carried out, thereby appropriately increasing the proportion of the platinum group elements in the form of an oxidized platinum group element complex in the platinum group elements contained in the solution containing the platinum group elements, and further enabling the proportion of the platinum group elements adsorbed on the scavenger in the form of an oxidized platinum group element complex to be appropriately 50 mol% or more. In particular, according to the findings of the present inventors, when recovery treatment is started in the absence of either a metal-free oxidant or a complexing agent, there is a tendency that the proportion of platinum group elements in the form of oxidized platinum group element complexes in the platinum group element-containing solution cannot be efficiently increased even if the recovery treatment is carried out. However, by starting the recovery treatment of platinum group elements in the presence of a metal-free oxidant and a complexing agent and / or a scavenger, the proportion of substances in the form of oxidized platinum group element complexes in the platinum group element-containing solution can be appropriately increased as the recovery treatment proceeds.
[0068] In addition, the trapping agent may be present at the start of the recovery of the platinum group elements, or may be included in the reaction system by adding the agent to the reaction system after the start of the recovery of the platinum group elements. In addition, the following method may be adopted: the recovery of the platinum group elements may be started in a state where a metal-free oxidizing agent and a complexing agent are simultaneously present in a solution containing the platinum group elements, a solution in which the proportion of the platinum group element complex in an oxidized state is 50 mol% or more is prepared by reaction, such a solution is passed through a column filled with the trapping agent, and the platinum group elements are adsorbed on the trapping agent in a state where the proportion of the platinum group elements adsorbed in the form of the platinum group element complex in an oxidized state is 50 mol% or more in the platinum group elements adsorbed on the trapping agent to recover the platinum group elements.
[0069] The metal-free oxidant is not particularly limited as long as it functions as an oxidant and does not contain a metal, and examples thereof include iodine; peroxides such as hydrogen peroxide, peracetic acid, and perbenzoic acid; air, and oxygen. Among these, hydrogen peroxide, air, and oxygen are preferred.
[0070] When air or oxygen is used as a metal-free oxidant, it can be introduced by continuously blowing them into a solution containing platinum group elements under atmospheric pressure, or a method of pressing them under prescribed pressurized conditions can be adopted. The pressurized conditions in this case are preferably 0.2 to 10 MPa, more preferably 0.4 to 8 MPa, further preferably 0.5 to 5 MPa, and particularly preferably 0.7 to 2.5 MPa. In addition, when oxygen is used, it can be used in a state mixed with an inert gas such as nitrogen, and the oxygen concentration in this case is preferably 0.2 to 90% by volume, more preferably 0.4 to 70% by volume, further preferably 1 to 50% by volume, and particularly preferably 2 to 12% by volume.
[0071] In addition, when a peroxide such as hydrogen peroxide is used as the metal-free oxidant, the amount of the peroxide such as hydrogen peroxide is preferably 0.5 to 200 mole times, more preferably 1 to 150 mole times, further preferably 2 to 100 mole times, and particularly preferably 5 to 50 mole times, relative to the molar amount of the platinum group element contained in the solution containing the platinum group element. At least a portion of the total amount of the metal-free oxidant used in the recovery process may be present at the time of starting the recovery process of the platinum group element, and additional addition may be performed after starting the recovery process of the platinum group element.
[0072] The complexing agent is not particularly limited as long as it has a complexing ability with the platinum group element and can form an oxidized complex, but a complexing agent represented by the following general formula (1) is preferred.
[0073] C n H m N p O q X r (1)
[0074] (In the above general formula (1), X is an element other than C, H, N, and O, n=1 to 13, m=1 to 18, p=0 to 4, q=0 to 4, r=0 to 4, and at least one of p and q is 1 or more).
[0075] In the above general formula (1), X includes S, P, halogen, etc. Among them, S is preferred. In addition, n is 1 to 13, preferably 2 to 12, more preferably 3 to 12, m is 1 to 18, preferably 2 to 18, more preferably 4 to 18, p is 0 to 4, preferably 0 to 2, q is 0 to 4, preferably 0 to 2, and r is 0 to 4, preferably 0 to 1.
[0076] Examples of the compound represented by the general formula (1) include organic ammonium salts such as ammonium acetate, amines such as ethylenediamine and triethylenetetramine, oximes such as dimethylglyoxime, imines such as bipyridine and phenanthroline, ketones such as acetylacetone and carbonamide, glycine, thiourea, 1-methylpiperazine, etc. Among these, organic ammonium salts, amines, and imines are preferred, and ammonium acetate, triethylenetetramine, and phenanthroline are preferred.
[0077] In addition, as a complexing agent, in addition to the compound shown in the above general formula (1), an inorganic ammonium salt is also preferably used. That is, any one of an organic ammonium salt and an inorganic ammonium salt can be preferably used. As the inorganic ammonium salt, ammonium halides can be cited, and as the ammonium halides, ammonium bromide, ammonium chloride, etc. are preferred.
[0078] The amount of the complexing agent is preferably 1 to 200 mole times relative to the molar amount of the platinum group element contained in the solution containing the platinum group element, more preferably 2 to 150 mole times, further preferably 3 to 100 mole times, and particularly preferably 20 to 80 mole times. By making the amount of the complexing agent in the above range, the recovery of the platinum group element can be carried out with higher efficiency. In addition, the complexing agent can be present at least a part of the total amount used in the recovery process at the moment of starting the recovery process of the platinum group element, and can be added after starting the recovery process of the platinum group element. From the viewpoint of recovering the platinum group element with higher efficiency, it is desired that the total amount used in the recovery process exists at the moment of starting the recovery process of the platinum group element.
[0079] In addition, as a capture agent, as long as it has the capture ability or adsorption ability of platinum group elements, it is not particularly limited, and resin, silica, carbon black, etc. can be cited. From the viewpoint of capture ability or adsorption ability, silica is preferred, and surface-treated silica is particularly preferred. As surface-treated silica, thiol-modified silica, silanol-modified silica, amine-modified silica, thiourea-modified silica, phosphoric acid-modified silica, carbamate-modified silica, etc. can be cited. Among these, thiol-modified silica, silanol-modified silica, and amine-modified silica are preferred.
[0080] The amount of the trapping agent is preferably 1 to 500 times by weight relative to the weight of the platinum group elements contained in the solution containing the platinum group elements, more preferably 2 to 300 times by weight, further preferably 5 to 100 times by weight, and particularly preferably 35 to 65 times by weight. By making the amount of the trapping agent within the above range, the platinum group elements can be recovered with higher efficiency. In addition, at least a portion of the total amount of the trapping agent used in the recovery process is present at the time of starting the recovery process of the platinum group elements, and additional additions can be made after starting the recovery process of the platinum group elements. From the viewpoint of recovering the platinum group elements with higher efficiency, it is desirable that the total amount used in the recovery process is present at the time of starting the recovery process of the platinum group elements.
[0081] The recovery treatment time in the recovery method of the present invention is not particularly limited, but is preferably 1 to 96 hours, more preferably 2 to 48 hours, and even more preferably 4 to 24 hours. By setting the recovery treatment time within the above range, platinum group elements can be recovered more efficiently at a high recovery rate.
[0082] Moreover, in the recovery method of the present invention, the recovery treatment of the platinum group elements is started in a state where a metal-free oxidant, a complexing agent and a scavenging agent are simultaneously present, and after the recovery treatment, the solution after the recovery treatment is filtered, etc., thereby recovering (filtering out) the scavenging agent adsorbed with the platinum group elements and separating it from the solution after the recovery treatment, thereby enabling the platinum group elements to be recovered in a state where they are adsorbed on the scavenging agent.
[0083] According to the recovery method of the present invention, the proportion of the platinum group elements adsorbed in the form of the platinum group element complex in the platinum group elements adsorbed on the capture agent is 50% mol or more, so that the platinum group elements can be recovered at a high recovery rate, thereby the platinum group elements can be appropriately provided for reuse at a high reuse rate. In addition, according to the recovery method of the present invention, the platinum group elements can be recovered at a high recovery rate, so the removal rate of the platinum group elements in the solution containing the platinum group elements can be improved. Therefore, for example, as a solution containing platinum group elements, by providing a solution containing a polymer, more specifically a solution of a hydrogenated conjugated diene rubber such as hydrogenated nitrile rubber, to the recovery treatment of the present invention, a hydrogenated conjugated diene rubber (polymer) such as hydrogenated nitrile rubber with a reduced content of platinum group elements can be provided. In particular, in hydrogenated conjugated diene rubbers (polymers) such as hydrogenated nitrile rubber, by reducing the content of platinum group elements, the coloring caused by the platinum group elements can be efficiently suppressed while making the mechanical strength such as tensile strength good.
[0084] Example
[0085] The present invention is described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. In the following, "parts" are by weight unless otherwise specified. The test or evaluation methods for physical properties and characteristics are as follows.
[0086] <Iodine value>
[0087] The iodine value of the hydrogenated nitrile rubber is measured in accordance with JIS K6235.
[0088] <Mooney viscosity>
[0089] The Mooney viscosity (polymer Mooney viscosity) of the hydrogenated nitrile rubber is measured at 100° C. in accordance with JIS K6300.
[0090] <Palladium content>
[0091] The palladium content was determined by atomic absorption spectrometry.
[0092] The atomic absorption spectrometer used for the measurement was ZA-3000 manufactured by Hitachi High-Technologies Corporation, and a furnace method and a flame method were appropriately utilized.
[0093] <Measurement of the ratio based on the valence of palladium>
[0094] The dried capture agent was attached to a substrate such as a metal plate and measured by XAFS (SPring-8 BL14B2). The valence was confirmed by the measurement results, and the ratio of each valence of palladium adsorbed on the capture agent was obtained by fitting. The measurement was carried out under the conditions of Pd K end 24155-24715eV, fluorescence yield method, Si (311), scanning: 32 minutes / sample.
[0095] <Preparation Example 1 (Preparation of Hydrogenated Nitrile Rubber Solution 1)>
[0096] In a reactor, 0.2 parts of sodium carbonate were dissolved in 200 parts of ion exchange water, and 2.3 parts of potassium soap of fatty acid (potassium salt of fatty acid) were added thereto to prepare a soap aqueous solution. Then, 38 parts of acrylonitrile and 0.45 parts of tert-dodecyl mercaptan (molecular weight modifier) were added to the soap aqueous solution in sequence, the internal gas was replaced with nitrogen three times, and then 62 parts of 1,3-butadiene were added. Next, the reactor was kept at 5°C, 0.1 parts of cumene hydroperoxide (polymerization initiator), appropriate amounts of reducing agent and chelating agent were added to initiate the polymerization reaction. Then, at the moment when the polymerization conversion rate reached 80%, 0.05 parts of 1% by weight aqueous solution of hydroquinone (polymerization terminator) and 0.05 parts of N-isopropylhydroxylamine (polymerization terminator) were added to terminate the polymerization reaction, 0.4 parts of alkylated phenol compound were added, and residual monomers were removed using a rotary evaporator at a water temperature of 60°C, thereby obtaining a latex of nitrile rubber (solid content concentration of about 25% by weight). The pH of the obtained latex was 9.6.
[0097] Next, the latex of the acrylonitrile-butadiene rubber obtained above was added to an aqueous solution of aluminum sulfate in an amount of 3% by weight relative to the acrylonitrile-butadiene rubber component in the latex obtained above, and stirred to coagulate the latex, and filtered out while washing with water and an alkaline aqueous solution, and then vacuum dried at 60° C. for 12 hours to obtain a solid acrylonitrile-butadiene rubber. Then, the obtained solid acrylonitrile-butadiene rubber was dissolved in acetone in a concentration of 14% by weight, loaded into an autoclave, and a silica-supported palladium catalyst (a catalyst formed by supporting palladium metal on silica) of 500 ppm by weight relative to the acrylonitrile-butadiene rubber was added, and a hydrogenation reaction was carried out at a hydrogen pressure of 3.0 MPa.
[0098] After the hydrogenation reaction is completed, the reaction system is cooled to room temperature and the hydrogen in the system is replaced with nitrogen. Then, the solution of the hydrogenated nitrile rubber obtained by the hydrogenation reaction is filtered to recover the silica-supported palladium catalyst, and the obtained filtrate is used as the hydrogenated nitrile rubber solution 1 of the sample used during the catalyst recovery process.
[0099] Take a part in the obtained hydrogenated nitrile rubber solution 1, put it into the water of 10 times the amount, polymer is precipitated, the obtained polymer is dried 24 hours with vacuum drying machine, thus obtain solid hydrogenated nitrile rubber. The composition of hydrogenated nitrile rubber is 36 weight % of acrylonitrile unit, 74 weight % of butadiene unit (including saturated part), iodine value is 8, and polymer Mooney viscosity [ML1+4, 100 ℃] is 63. For the obtained solid hydrogenated nitrile rubber, the palladium metal amount in the hydrogenated nitrile rubber is measured by atomic absorption spectrometry, and the palladium metal amount is 250 weight ppm as a result. According to this result, it can be said that the palladium metal amount in the hydrogenated nitrile rubber solution 1 is 250 weight ppm.
[0100] <Preparation Example 2 (Preparation of Hydrogenated Nitrile Rubber Solution 2)>
[0101] The amount of the silica-supported palladium catalyst was changed to 400 ppm by weight based on the amount of palladium metal, and polymerization and hydrogenation reactions were carried out in the same manner as in Preparation Example 1. Then, the solution of hydrogenated nitrile rubber obtained by the hydrogenation reaction was filtered to recover the silica-supported palladium catalyst, and the obtained filtrate was used as a hydrogenated nitrile rubber solution 2 of a sample used in the catalyst recovery process.
[0102] Take a part in the obtained hydrogenated nitrile rubber solution 2, measure in the same manner as Example 1, the composition of the result hydrogenated nitrile rubber is acrylonitrile unit 36 % by weight, divinyl unit (comprising the part of saturation) 74 % by weight, iodine value is 9, and polymer Mooney viscosity [ML1+4,100 ℃] is 62.For the obtained solid hydrogenated nitrile rubber, measure the palladium metal amount in the hydrogenated nitrile rubber by atomic absorption spectrometry, and the palladium metal amount is 190 ppm by weight as a result.According to this result, it can be said that the palladium metal amount in the hydrogenated nitrile rubber solution 2 is 190 ppm by weight.
[0103] <Preparation Example 3 (Preparation of Hydrogenated Nitrile Rubber Solution 3)>
[0104] The amount of the silica-supported palladium catalyst was changed to 330 ppm by weight based on the amount of palladium metal, and polymerization and hydrogenation reactions were carried out in the same manner as in Preparation Example 1. Then, the solution of hydrogenated nitrile rubber obtained by the hydrogenation reaction was filtered to recover the silica-supported palladium catalyst, and the obtained filtrate was used as a hydrogenated nitrile rubber solution 3 of a sample used in the catalyst recovery process.
[0105] Take a part in the obtained hydrogenated nitrile rubber solution 3, measure in the same manner as Example 1, the composition of the result hydrogenated nitrile rubber is acrylonitrile unit 36 % by weight, divinyl unit (comprising the part of saturation) 74 % by weight, iodine value is 12, and polymer Mooney viscosity [ML1+4,100 ℃] is 59.For the obtained solid hydrogenated nitrile rubber, measure the palladium metal amount in the hydrogenated nitrile rubber by atomic absorption spectrometry, and the palladium metal amount is 160 ppm by weight as a result.According to this result, it can be said that the palladium metal amount in the hydrogenated nitrile rubber solution 3 is 160 ppm by weight.
[0106] <Preparation Example 4 (Preparation of Hydrogenated Nitrile Rubber Solution 4)>
[0107] Polymerization was carried out in the same manner as in Manufacturing Example 1 to obtain a latex of acrylonitrile-butadiene rubber. Then, the obtained latex of acrylonitrile-butadiene rubber was coagulated, washed with water and dried in the same manner as in Example 1 to obtain a solid acrylonitrile-butadiene rubber, which was dissolved in acetone to obtain an acetone solution of acrylonitrile-butadiene rubber having a concentration of 15% by weight.
[0108] Next, in a reactor different from the above, 1 part of palladium acetate, 3 parts of polymethylvinyl ether, and 3 parts of hydrazine (10 wt % aqueous solution) were mixed in 800 parts of acetone to obtain a palladium acetate catalyst solution.
[0109] Then, in the acetone solution of the acrylonitrile-butadiene rubber obtained above, add the solution of the palladium acetate catalyst of the above-mentioned preparation with respect to the acrylonitrile-butadiene rubber as 250 ppm by weight with respect to the palladium metal amount, and put it in the autoclave with stirrer, circulate nitrogen 10 minutes, thus remove dissolved oxygen. Then, after the system inside is replaced with hydrogen twice, the hydrogen of 5MPa of pressurization makes content be warming up to 50 ℃ and stir 6 hours, thus carry out hydrogenation reaction, obtain the acetone solution of hydrogenated acrylonitrile-butadiene rubber. Then, the hydrogenated acrylonitrile-butadiene rubber solution 4 of the sample used when the acetone solution of the obtained hydrogenated acrylonitrile-butadiene rubber is used as the catalyst recovery process.
[0110] Take a part in the obtained hydrogenated nitrile rubber solution 4, measure in the same manner as Example 1, the composition of the result hydrogenated nitrile rubber is acrylonitrile unit 36 % by weight, divinyl unit (comprising the part of being saturated) 74 % by weight, iodine value is 7.4, and polymer Mooney viscosity [ML1+4,100 ℃] is 65.For the obtained solid hydrogenated nitrile rubber, measure the palladium metal amount in the hydrogenated nitrile rubber by atomic absorption spectrometry, and the palladium metal amount is 250 ppm by weight as a result.According to this result, it can be said that the palladium metal amount in the hydrogenated nitrile rubber solution 4 is 250 ppm by weight.
[0111] <Preparation Example 5 (Preparation of Hydrogenated Nitrile Rubber Solution 5)>
[0112] In a reactor, 0.2 parts of sodium carbonate were dissolved in 200 parts of ion exchange water, and 2.25 parts of potassium soap (potassium salt of fatty acid) were added thereto to prepare a soap solution. Then, 13 parts of acrylonitrile, 49 parts of n-butyl acrylate and 0.45 parts of tert-dodecyl mercaptan (molecular weight modifier) were added to the soap solution, the internal gas was replaced with nitrogen three times, and then 21 parts of 1,3-butadiene were added. Next, the reactor was kept at 5°C, 0.1 parts of cumene hydroperoxide (polymerization initiator), appropriate amounts of reducing agent and chelating agent were added to initiate the polymerization reaction. When the reaction conversion rate reached 60%, 8 parts of acrylonitrile and 9 parts of 1,3-butadiene were added. When the polymerization conversion rate reached 85%, 0.05 parts of a 10 wt% aqueous solution of hydroquinone (polymerization terminator) and 0.05 parts of N-isopropylhydroxylamine (polymerization terminator) were added to terminate the polymerization reaction. 0.45 parts of an alkylated phenol compound were added, and then a rotary evaporator with a water temperature of 60° C. was used to remove the residual monomers to obtain a latex of nitrile rubber (solid content concentration of about 25 wt%). In addition, the pH of the obtained latex was 10.1.
[0113] Next, the latex of the acrylonitrile-butadiene rubber obtained above was added to an aqueous solution of aluminum sulfate in an amount of 3% by weight relative to the acrylonitrile-butadiene rubber component of the latex obtained above, and stirred to coagulate the latex, and filtered out while washing with water and an alkaline aqueous solution, and then vacuum dried at 60° C. for 12 hours to obtain a solid acrylonitrile-butadiene rubber. Then, the obtained solid acrylonitrile-butadiene rubber was dissolved in acetone in a concentration of 12% by weight, loaded into an autoclave, and a silica-supported palladium catalyst (a catalyst formed by supporting palladium metal on silica) of 500 ppm by weight relative to the acrylonitrile-butadiene rubber was added, and a hydrogenation reaction was carried out at a hydrogen pressure of 3.0 MPa.
[0114] After the hydrogenation reaction is completed, the reaction system is cooled to room temperature and the hydrogen in the system is replaced with nitrogen. Then, the solution of the hydrogenated nitrile rubber obtained by the hydrogenation reaction is filtered to reclaim the silica-supported palladium catalyst, and the resulting filtrate is used as the hydrogenated nitrile rubber solution 5 of the sample used during the catalyst recovery process.
[0115] Take a part in the obtained hydrogenated nitrile rubber solution 5, measure in the same manner as Example 1, the composition of the result hydrogenated nitrile rubber is acrylonitrile unit 19 % by weight, divinyl unit (comprising the part of being saturated) 38 % by weight, 43 % by weight of n-butyl acrylate unit, iodine value is 10.9, and polymer Mooney viscosity [ML1+4,100 ℃] is 43.For the obtained solid hydrogenated nitrile rubber, measure the palladium metal amount in the hydrogenated nitrile rubber by atomic absorption spectrometry, and the palladium metal amount is 250 ppm by weight as a result.According to this result, it can be said that the palladium metal amount in the hydrogenated nitrile rubber solution 5 is 250 ppm by weight.
[0116] <Example 1>
[0117] The hydrogenated nitrile rubber solution 1 obtained in the preparation example 1 is added to a pressure-resistant container with a stirring device, in which a mercaptan-modified silica (trade name "SH SILICA", manufactured by Fuji Silicon Chemical Co., Ltd., the same below) as a trapping agent is added in a weight ratio of 50 times relative to the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1. Then, in this solution, triethylenetetramine (hereinafter, appropriately referred to as "TETA") as a complexing agent is added in a molar ratio of 60 times relative to the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1. Then, after being pressurized to 1MPa with 7% by volume of oxygen, the temperature is raised to 55°C by heating, and the pressure is continued with oxygen while stirring at 55°C for 24 hours. After the reaction is completed, the mercaptan-modified silica is recovered from the reaction mixture by filtration, thereby carrying out a catalyst recovery process.
[0118] The obtained filtrate is put into 10 times the amount of water, so that the rubber component is separated out, the obtained rubber component is taken out, and vacuum drying is performed for 24 hours with a vacuum dryer to obtain hydrogenated nitrile rubber. The amount of palladium metal in the obtained hydrogenated nitrile rubber is 70 ppm by weight. In addition, the mercaptan-modified silica recovered by filtration is cleaned with acetone, and the rubber component attached is removed thereby. Then, after drying, a part of the mercaptan-modified silica after drying is used, and XAFS is performed according to the above method to measure, and the weight ratio of palladium in the palladium recovered by mercaptan-modified silica, which is a divalent or higher oxidation state, is obtained. The results are shown in Table 1. In addition, a part of the mercaptan-modified silica after drying is used to carry out wet decomposition, and a determination solution is obtained, and atomic absorption spectrometry is performed, and the amount of palladium metal captured and recovered by mercaptan-modified silica as a trapping agent is measured thereby, and the result is 155 ppm by weight per unit weight of hydrogenated nitrile rubber.
[0119] Then, according to the palladium metal amount (250 ppm by weight) of the hydrogenated nitrile rubber before the catalyst recovery process, the palladium metal amount (70 ppm by weight) in the hydrogenated nitrile rubber after the catalyst recovery process and the palladium metal amount (155 ppm by weight) captured and recovered by the trapping agent (mercaptan-modified silica), the catalyst removal rate and the catalyst recovery rate were calculated according to the following formula. The results are shown in Table 1.
[0120] Catalyst removal rate (%) = [(the amount of palladium metal in hydrogenated nitrile rubber before catalyst recovery treatment - catalyst
[0121] (amount of palladium metal in hydrogenated nitrile rubber after catalyst recovery treatment) / (amount of palladium metal in hydrogenated nitrile rubber before catalyst recovery treatment)
[0122] Palladium metal content of nitrile rubber] × 100
[0123] Catalyst recovery rate (%) = (palladium captured and recovered by the capture agent (thiol-modified silica)
[0124] amount of palladium metal / the amount of palladium metal in hydrogenated nitrile rubber before catalyst recovery treatment)×100
[0125] <Example 2>
[0126] The hydrogenated nitrile rubber solution 2 obtained in Preparation Example 2 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, the silanol-modified silica in the amount shown in Table 1 was used to replace the thiol-modified silica, the amount of triethylenetetramine was set to the amount shown in Table 1, 8 volume % of oxygen was used to replace 7 volume % of oxygen, and the reaction time was set to the time shown in Table 1. Otherwise, the catalyst recovery treatment was carried out in the same manner as in Example 1.
[0127] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 67 ppm by weight.In addition, for the silanol-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1.And then, measure the palladium metal amount captured, recovered by silanol-modified silica in the same manner as Example 1, and the result is 112 ppm by weight with the weight of per unit hydrogenated nitrile rubber.The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0128] <Example 3>
[0129] The hydrogenated nitrile rubber solution 2 obtained in Preparation Example 2 was used instead of the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, amine-modified silica (trade name "NH SILICA", manufactured by Fuji Silicon Chemical Co., Ltd., the same below) in the amount shown in Table 1 was used instead of the thiol-modified silica, the amount of triethylenetetramine used was set to the amount shown in Table 1, 7 volume % of oxygen was not used, but hydrogen peroxide water was used instead, and the amount of hydrogen peroxide water was set to 15 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in terms of molar ratio, and stirred at 55° C. for 3 hours, and then hydrogen peroxide water was further added in an amount of 15 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in terms of molar ratio, and the reaction time was set to the time shown in Table 1. The catalyst recovery treatment was carried out in the same manner as in Example 1, except that the reaction time was set to the time shown in Table 1.
[0130] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 44 ppm by weight. In addition, for the amine-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by amine-modified silica in the same manner as Example 1, and the result is 130 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0131] <Example 4>
[0132] The amount of triethylenetetramine used was changed to the amount shown in Table 1, and the amount of hydrogen peroxide added was set to 0.12 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in terms of molar ratio. 0.12 times the amount of hydrogen peroxide was added, and then the temperature was raised to 55° C. by heating, and hydrogen peroxide was continuously added every minute in an amount of 0.12 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in terms of molar ratio while stirring at 55° C. for 6 hours. Except for this, the catalyst recovery treatment was carried out in the same manner as in Example 3.
[0133] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 48 ppm by weight. In addition, for the amine-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by amine-modified silica in the same manner as Example 1, and the result is 132 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0134] <Example 5>
[0135] The hydrogenated nitrile rubber solution 3 obtained in Preparation Example 3 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, the amine-modified silica in the amount shown in Table 1 was used to replace the thiol-modified silica, the ammonium bromide in the amount shown in Table 1 was used to replace triethylenetetramine, and instead of using 7 volume % of oxygen, hydrogen peroxide was used instead, and the amount thereof was set to 30 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 3 in terms of molar ratio, and the reaction time was set to the time shown in Table 1. Except for this, the catalyst recovery treatment was carried out in the same manner as in Example 1.
[0136] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 20 ppm by weight. In addition, for the amine-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by amine-modified silica in the same manner as Example 1, and the result is 115 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0137] <Example 6>
[0138] The catalyst recovery treatment was carried out in the same manner as in Example 1 except that ammonium chloride in an amount shown in Table 1 was used instead of triethylenetetramine, 7 volume % of oxygen was not used but was replaced by hydrogen peroxide water, and the amount thereof was set to 15 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in terms of molar ratio, and the reaction time was set to the time shown in Table 1.
[0139] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 25 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 206 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0140] <Example 7>
[0141] The hydrogenated nitrile rubber solution 2 obtained in Preparation Example 2 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, and the amount of phenanthroline shown in Table 1 was used to replace triethylenetetramine. Instead of using 7% by volume of oxygen, hydrogen peroxide was used instead, and its amount was set to 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in a molar ratio. The mixture was stirred at 55° C. for 3 hours, and then hydrogen peroxide was further added in an amount that was 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in a molar ratio. The reaction time was set to the time shown in Table 1. Except for this, the catalyst recovery treatment was carried out in the same manner as in Example 1.
[0142] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 65 ppm by weight. In addition, for the mercaptan-modified silica obtained by recovery, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 130 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0143] In Example 7, the catalyst removal rate and the catalyst recovery rate showed different values due to the influence of measurement error, but they can be judged to be substantially the same values (the same is true for Examples 8, 9, 11, and 12).
[0144] <Example 8>
[0145] The catalyst recovery treatment was carried out in the same manner as in Example 4 except that phenanthroline in the amount shown in Table 1 was used instead of triethylenetetramine, and silanol-modified silica in the amount shown in Table 1 was used instead of amine-modified silica.
[0146] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 59 ppm by weight.In addition, for the silanol-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1.And then, measure the palladium metal amount captured, recovered by silanol-modified silica in the same manner as Example 1, and the result is 138 ppm by weight with the weight of per unit hydrogenated nitrile rubber.The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0147] <Example 9>
[0148] The hydrogenated nitrile rubber solution 2 obtained in Preparation Example 2 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, and the amount of phenanthroline shown in Table 1 was used to replace triethylenetetramine. 7% by volume of oxygen was supplied by continuously blowing it at normal pressure in an open system instead of supplying it under a pressurized condition of 1 MPa, and the reaction time was set to the time shown in Table 1. Otherwise, the catalyst recovery treatment was carried out in the same manner as in Example 1.
[0149] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 42 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 152 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0150] <Example 10>
[0151] The catalyst recovery treatment was carried out in the same manner as in Example 5 except that phenanthroline in the amount shown in Table 1 was used instead of ammonium bromide, the amount of hydrogen peroxide solution used was set to the amount shown in Table 1, and mercaptan-modified silica in the amount shown in Table 1 was used instead of amine-modified silica.
[0152] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 39 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 120 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0153] <Example 11>
[0154] The catalyst recovery treatment was carried out in the same manner as in Example 5, except that the amount of ammonium acetate shown in Table 1 was used instead of ammonium bromide, the amount of hydrogen peroxide water used was set to the amount shown in Table 1, the amount of silanol-modified silica shown in Table 1 was used instead of amine-modified silica, and the reaction time was set to the time shown in Table 1.
[0155] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 53 ppm by weight.In addition, for the silanol-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1.And then, measure the palladium metal amount captured, recovered by silanol-modified silica in the same manner as Example 1, and the result is 113 ppm by weight with the weight of per unit hydrogenated nitrile rubber.The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0156] <Example 12>
[0157] The catalyst recovery treatment was carried out in the same manner as in Example 1 except that the amount of silanol-modified silica shown in Table 1 was used instead of mercaptan-modified silica, the amount of ammonium acetate shown in Table 1 was used instead of triethylenetetramine, 7% by volume of oxygen was not used but was replaced by hydrogen peroxide water in an amount that was 15 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in terms of molar ratio, and the reaction time was set to the time shown in Table 1.
[0158] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 83 ppm by weight.In addition, for the silanol-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium of the oxidation state above divalent, the results are shown in Table 1.And then, measure the palladium metal amount captured, recovered by silanol-modified silica in the same manner as Example 1, the result is 174 ppm by weight with the weight of per unit hydrogenated nitrile rubber.The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0159] <Example 13>
[0160] The catalyst recovery process was carried out in the same manner as in Example 1 except that the hydrogenated nitrile rubber solution 4 obtained in Preparation Example 4 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, the ammonium chloride in the amount shown in Table 1 was used to replace triethylenetetramine, and 8 volume % of oxygen was used to replace 7 volume % of oxygen.
[0161] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 55 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 132 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0162] <Example 14>
[0163] The hydrogenated nitrile rubber solution 5 obtained in Preparation Example 5 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, and the ammonium chloride in the amount shown in Table 1 was used to replace triethylenetetramine. Instead of using 7% by volume of oxygen, hydrogen peroxide was used instead, and the amount thereof was set to 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 5 in a molar ratio. The mixture was stirred at 55° C. for 3 hours, and then hydrogen peroxide was further added in an amount that was 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 5 in a molar ratio. The reaction time was set to the time shown in Table 1. Except for this, the catalyst recovery treatment was carried out in the same manner as in Example 1.
[0164] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 43 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 180 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0165] <Example 15>
[0166] The hydrogenated nitrile rubber solution 2 obtained in Preparation Example 2 was used to replace the hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1, mercaptan-modified silica was not added as a scavenger, ammonium acetate in an amount shown in Table 1 was used to replace triethylenetetramine, 7% by volume of oxygen was not used, but hydrogen peroxide was used instead, and its amount was set to 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in a molar ratio, stirred at 55° C. for 3 hours, and then hydrogen peroxide was further added in an amount of 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 2 in a molar ratio, and the reaction time was set to the time shown in Table 1. Except for this, the catalyst recovery treatment was carried out in the same manner as in Example 1. Then, the hydrogenated nitrile rubber solution after the catalyst recovery treatment was passed through a column filled with a thiourea-modified ion exchange resin (scavenger).
[0167] Then, use the solution obtained after by liquid, obtain hydrogenated nitrile rubber in the same manner as Example 1, and the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 45 ppm by weight.In addition, for the thiourea modified ion exchange resin in the post, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium of the oxidation state above divalent, and the results are shown in Table 1.And then, measure the palladium metal amount captured, recovered by thiourea modified ion exchange resin in the same manner as Example 1, and the result is counted as 124 ppm by weight with the weight of per unit hydrogenated nitrile rubber.The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0168] <Comparative Example 1>
[0169] The hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1 is added to a pressure-resistant container with a stirring device, and triethylenetetramine as a complexing agent is added to the solution in an amount of 10 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in a molar ratio. Then, hydrogen peroxide is added in an amount of 20 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in a molar ratio. Then, the temperature is raised to 55°C by heating the solution, stirred at 55°C for 5 hours, and then thiol-modified silica as a capture agent is added in a weight ratio of 50 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1, and further stirred at 55°C for 2 hours. After the reaction is completed, the thiol-modified silica is recovered from the reaction mixture by filtration, thereby performing a catalyst recovery process.
[0170] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 112 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is 75 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0171] <Comparative Example 2>
[0172] The hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1 is added to a pressure-resistant container with a stirring device, and a mercaptan-modified silica as a capture agent is added to the solution in a weight ratio of 50 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1. Then, dimethylglyoxime as a complexing agent in a molar ratio of 40 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 is added to the solution. Then, after adding hydrogen peroxide in a molar ratio of 20 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1, the solution is heated, thereby heating to 55°C and stirring at 55°C for 6 hours. After the reaction is completed, the mercaptan-modified silica is recovered from the reaction mixture by filtration, thereby performing a catalyst recovery process.
[0173] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 237 ppm by weight. In addition, for the mercaptan-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by mercaptan-modified silica in the same manner as Example 1, and the result is calculated as 12 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0174] <Comparative Example 3>
[0175] The hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1 was added to a pressure-resistant container with a stirring device. After the solution was opened and 7% by volume of oxygen was blown in at normal pressure, it was heated to 55°C, and stirred at 55°C for 3 hours while continuing to blow in oxygen. After 3 hours of stirring, ammonium bromide was added in an amount of 40 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in a molar ratio, and stirred at 55°C for further 3 hours while continuing to blow in oxygen. Then, silanol-modified silica was added to the solution in an amount of 50 times the weight of the palladium metal contained in the hydrogenated nitrile rubber solution 1 in a weight ratio, and stirred at 55°C for further 2 hours while continuing to pressurize with oxygen. After the reaction was completed, the silanol-modified silica was recovered from the reaction mixture by filtration, thereby performing a catalyst recovery process.
[0176] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 172 ppm by weight. In addition, for the silanol-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1. And then, measure the palladium metal amount captured, recovered by silanol-modified silica in the same manner as Example 1, and the result is calculated as 15 ppm by weight with the weight of per unit hydrogenated nitrile rubber. The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0177] <Comparative Example 4>
[0178] The hydrogenated nitrile rubber solution 1 obtained in Preparation Example 1 was added to a pressure-resistant container with a stirring device, and hydrogen peroxide was added in an amount of 20 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in a molar ratio, and stirred at 55°C for 3 hours. After 3 hours of stirring, ammonia water was added in an amount of 30 times the amount of palladium metal contained in the hydrogenated nitrile rubber solution 1 in a molar ratio, and further stirred at 55°C for 2 hours. Then, silanol-modified silica was added to the solution in an amount of 50 times the weight of the palladium metal contained in the hydrogenated nitrile rubber solution 1 in a weight ratio, and further stirred at 55°C for 2 hours. After the reaction was completed, the silanol-modified silica was recovered from the reaction mixture by filtration, thereby performing a catalyst recovery process.
[0179] Then, obtain hydrogenated nitrile rubber in the same manner as Example 1, the palladium metal amount in the hydrogenated nitrile rubber obtained as a result is 90 ppm by weight.In addition, for the silanol-modified silica recovered, carry out XAFS measurement in the same manner as Example 1, obtain the weight ratio of the palladium in the oxidation state above divalent, and the results are shown in Table 1.And then, measure the palladium metal amount captured, recovered by silanol-modified silica in the same manner as Example 1, and the result is calculated as 12 ppm by weight with the weight of per unit hydrogenated nitrile rubber.The catalyst removal rate and the catalyst recovery rate obtained by these results are shown in Table 1.
[0180] [Table 1]
[0181]
[0182] In Table 1, the amount of oxidant used represents the molar multiple of the amount of palladium contained in the hydrogenated nitrile rubber solution or the injection condition of oxygen, the amount of complexing agent used represents the molar multiple of the amount of palladium contained in the hydrogenated nitrile rubber solution, and the amount of scavenger used represents the weight multiple of the amount of palladium contained in the hydrogenated nitrile rubber solution.
[0183] Table 1 shows the ratio of the platinum group elements adsorbed in the form of platinum group element complexes in divalent or higher oxidation states, but the ratio of the platinum group elements adsorbed in the form of platinum group element complexes in oxidation states including monovalent oxidation states is the same value.
[0184] As shown in Table 1, when the proportion of platinum group elements adsorbed in the form of oxidized platinum group element complexes in the platinum group elements adsorbed on the capture agent (the proportion of platinum group elements adsorbed in the form of platinum group element complexes in divalent or higher oxidation states) is 50 mol% or more, and the platinum group elements are adsorbed on the capture agent to recover the platinum group elements, the capture rate of the capture agent is high, the platinum group elements can be recovered at a high recovery rate, and the removal rate of the platinum group elements from the hydrogenated nitrile rubber solution is also high (Examples 1 to 15).
[0185] On the other hand, when the proportion of platinum group elements adsorbed in the form of platinum group element complexes in an oxidized state (the proportion of platinum group elements adsorbed in the form of platinum group element complexes in a divalent or higher oxidation state) among the platinum group elements adsorbed on the capture agent is less than 50 mol%, the capture rate of the capture agent is low and the recovery of the platinum group elements is low (Comparative Examples 1 to 4).
Claims
1. A method for recovering platinum group elements, which is a method for recovering platinum group elements from a solution containing platinum group elements by using a capture agent to adsorb the platinum group elements to the capture agent. The platinum group elements are adsorbed on the trapping agent to recover the platinum group elements in a state where the ratio of the platinum group elements adsorbed in the form of an oxidized platinum group element complex among the platinum group elements adsorbed on the trapping agent is 50 mol% or more.
2. The method for recovering platinum group elements according to claim 1, wherein: The platinum group elements are adsorbed on the trapping agent to recover the platinum group elements in a state where the proportion of the platinum group elements adsorbed in the form of a platinum group element complex in a divalent or higher oxidation state is 50 mol% or more.
3. The method for recovering platinum group elements according to claim 1 or 2, wherein: Recovering platinum group elements in the presence of a complexing agent represented by the following general formula (1), CnHmNpOqX(1) In the general formula (1), X is an element other than C, H, N, and O, n=1 to 13, m=1 to 18, p=0 to 4, q=0 to 4, r=0 to 4, and at least one of p and q is 1 or more.
4. The method for recovering platinum group elements according to any one of claims 1 to 3, wherein: The complexing agent is an ammonium salt, an amine or an imine.
5. The method for recovering platinum group elements according to any one of claims 1 to 4, wherein: The solution containing platinum group elements is a solution containing platinum group elements and a polymer.
6. The method for recovering platinum group elements according to claim 5, wherein: The solution containing platinum group elements is a solution containing hydrogenated nitrile rubber and platinum group elements from a platinum group element-containing catalyst.
7. The method for recovering platinum group elements according to any one of claims 1 to 6, wherein: In a state where the metal-free oxidizing agent, the complexing agent, and the scavenging agent are simultaneously in contact with the solution containing the platinum group element, the platinum group element contained in the solution containing the platinum group element is adsorbed to the scavenging agent, thereby starting recovery.
8. The method for recovering platinum group elements according to any one of claims 1 to 6, characterized in that: The metal-free oxidizing agent and the complexing agent are simultaneously contacted with a solution containing a platinum group element, and the solution containing a platinum group element complex in an oxidized state of 50 mol% or more is passed through a column filled with a trapping agent to adsorb the platinum group element to the trapping agent.
9. The method for recovering platinum group elements according to claim 7 or 8, wherein: The metal-free oxidizing agent is hydrogen peroxide, air or oxygen.
10. The method for recovering platinum group elements according to any one of claims 1 to 9, wherein: The capture agent is surface treated silica.