Composition for protecting copper surface, semiconductor intermediate using same, and method for producing

By using the copper surface protection composition to form a dense protective layer, the problem of copper surface oxidation in 3D integrated technology is solved, stable storage and efficient connection of semiconductor intermediates are achieved, and the feasibility of semiconductor manufacturing is improved.

CN118900935APending Publication Date: 2024-11-05MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027859.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-17
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In 3D integration technology, oxide generation on the copper surface hinders sufficient interconnection between semiconductors. Existing methods such as the use of metals with high oxidation potentials to hinder Cu oxidation, there are problems of waste of resources and inefficiency.

Method used

A copper surface protection composition is adopted, which comprises a copper surface protection agent, a solvent and a pH adjusting agent. By contacting the copper surface, a dense protective layer is formed to prevent oxygen from passing through, thereby preventing oxidation of the copper surface. The composition can be used to make semiconductor intermediates and remove efficiently when needed.

Benefits of technology

It effectively prevents oxidation of the copper surface, extends the storage time of semiconductor intermediates, and is suitable for semiconductor manufacturing in 3D integration technology due to its high removal ability and excellent useability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900935A_ABST
    Figure CN118900935A_ABST
Patent Text Reader

Abstract

Provided is a means for preventing oxidation of a copper surface. A composition for protecting a copper surface, which contains a solvent and at least one copper surface-protecting agent selected from the group consisting of compounds represented by formulae (1)-(3) and salts thereof, and a solvent. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copper surface protective composition, and a semiconductor intermediate and a semiconductor production method using the same. Background Art

[0002] In recent years, the miniaturization and high-performance of electronic components have been progressing, and the miniaturization and high-performance of semiconductors have been sought.

[0003] As a method to meet the requirements of miniaturization and high functionality of semiconductors, 3D integration technology has attracted attention. In 3D integration technology, multiple semiconductor chips or semiconductor wafers are connected to each other and stacked. As stacking forms, chip to chip (C2C), chip to wafer (C2W), wafer to wafer (W2W), etc. are known.

[0004] As such a 3D integration technology, for example, Patent Document 1 records an invention regarding a semiconductor structure comprising: a semiconductor layer, an adhesive layer arranged above the aforementioned semiconductor layer, an anode metal layer arranged above the aforementioned adhesive layer, and a cathode metal layer arranged above the aforementioned anode metal layer.

[0005] Patent Document 1 records that in interconnection based on Cu-Cu bonding, rapid oxide generation on the Cu surface will hinder sufficient interconnection, which is a major issue. In addition, Patent Document 1 records: as a method of hindering Cu oxidation, a metal (Mg, etc.) with an oxidation potential higher than that of Cu is used to form a galvanic pair, and Mg itself is sacrificed, thereby hindering or reducing the growth of Cu oxides.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2020-512703 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] In view of such a situation, a new means for preventing oxidation of the copper surface is sought.

[0011] Solutions for solving problems

[0012] The present invention includes the following aspects, for example.

[0013] [1] A copper surface protective composition comprising a copper surface protective agent and a solvent,

[0014] The copper surface protective agent is at least one selected from the group consisting of compounds represented by the following formulae (1) to (3) and salts thereof.

[0015]

[0016] [In formulas (1) to (3), R is a substituted or unsubstituted alkyl group having 3 to 30 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 30 carbon atoms]

[0017] [2] The copper surface protective composition according to [1] above, wherein the copper surface protective agent comprises a compound represented by formula (1) and / or a salt thereof.

[0018] [3] The copper surface protective composition according to [1] or [2], wherein R is a substituted or unsubstituted alkyl group having 3 to 30 carbon atoms.

[0019] [4] The copper surface protective composition according to any one of [1] to [3] above, further comprising a pH adjuster.

[0020] [5] The copper surface protective composition according to [4] above, wherein the pH adjuster comprises at least one selected from the group consisting of sodium hydroxide and potassium hydroxide.

[0021] [6] The copper surface protective composition according to any one of [1] to [5] above, wherein the pH thereof is 2.5 to 5.5.

[0022] [7] The copper surface protective composition according to any one of [1] to [6] above, which is used for the production of semiconductors.

[0023] [8] A method for producing a first semiconductor intermediate, comprising a copper-containing layer and a copper surface protection layer stacked on the copper-containing layer, the method comprising the following step (1):

[0024] The copper surface protective layer is formed by contacting the copper surface protective composition described in any one of [1] to [7] above on the copper surface protective layer in the first semiconductor having the copper surface protective layer.

[0025] [9] The method for producing the first semiconductor intermediate according to [8] above, comprising: before the step (1), a step of cleaning the copper-containing layer using a cleaning solution.

[0026]

[10] The method for producing a first semiconductor intermediate according to [9] above, wherein the cleaning solution contains at least one selected from the group consisting of hydrofluoric acid, sulfuric acid, nitric acid and ammonia.

[0027]

[11] A method for manufacturing a semiconductor, which is a method for manufacturing a semiconductor including a copper-containing bonding layer, the manufacturing method comprising:

[0028] A step of removing the copper surface protection layer of the first semiconductor intermediate produced by the method of any one of [8] to

[10] to expose the copper-containing layer; and

[0029] The step of bonding the exposed copper-containing layer to the metal-containing layer in the second semiconductor intermediate including the metal-containing layer to form a copper-containing bonding layer.

[0030] Effects of the Invention

[0031] According to the present invention, a copper surface protective composition that can prevent oxidation of the copper surface is provided. This can prevent oxidation of the copper surface of a semiconductor, and can produce semiconductors that are preferably interconnected in 3D integration technology. DETAILED DESCRIPTION

[0032] Hereinafter, the mode for carrying out the present invention will be described in detail.

[0033] <Copper Surface Protective Composition>

[0034] The copper surface protective composition comprises a copper surface protective agent and a solvent, wherein the copper surface protective agent is at least one selected from the group consisting of compounds represented by formulas (1) to (3) and their salts. The copper surface protective composition may further comprise a pH adjuster, a surfactant, a viscosity adjuster, a chelating agent, a reducing agent, a defoaming agent, etc. The copper surface protective composition is preferably used for manufacturing semiconductors.

[0035] According to the copper surface protection composition of the present invention, oxidation of the copper surface can be prevented. Specifically, by contacting the copper surface protection composition with a copper surface (e.g., a copper-containing layer possessed by a semiconductor), a copper surface protection layer can be formed. The copper surface protection layer is a dense layer, so it can prevent the penetration of oxygen. As a result, the contact between the copper surface and oxygen can be prevented, thereby preventing oxidation of the copper surface.

[0036] It should be noted that in 3D integration technology, since semiconductor intermediates having two interconnected copper-containing layers are separately manufactured and then stacked to manufacture semiconductors, the storage period of the semiconductor intermediate having the copper-containing layer may be prolonged. According to the surface protection composition of the present invention, the copper surface protection layer formed on the copper-containing layer can be kept stable for a long time, so the semiconductor intermediate having the above-mentioned copper surface protection layer can be stored for a long time.

[0037] In addition, in one embodiment, the copper surface protective layer formed by the copper surface protective composition has high removability, so it is excellent in usability. Since the copper-copper surface protective layer does not necessarily require a bonding force based on a covalent bond, the copper surface protective layer can be easily removed by heating, hydrogen ashing, ion irradiation of an inert gas, etc. Therefore, the copper surface protective composition has excellent usability.

[0038] [Copper surface protective agent]

[0039] The copper surface protective agent is selected from the group consisting of compounds represented by formulas (1) to (3) and salts thereof.

[0040]

[0041] In the above formulae (1) to (3), R is a substituted or unsubstituted alkyl group having 3 to 30 carbon atoms or a substituted or unsubstituted aryl group having 6 to 30 carbon atoms.

[0042] The alkyl group having 3 to 30 carbon atoms is not particularly limited, and examples thereof include propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, heptyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, octadecyl, and eicosyl.

[0043] When the alkyl group having 3 to 30 carbon atoms has a substituent, the substituent is not particularly limited, and examples thereof include alkoxy groups having 1 to 30 carbon atoms, such as methoxy, ethoxy, and propoxy; hydroxyl groups; cyano groups; nitro groups; halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms), etc. The substituent may be one or a combination of two or more.

[0044] Examples of the aryl group having 6 to 30 carbon atoms include phenyl, naphthyl, and anthracenyl.

[0045] When the aryl group having 6 to 30 carbon atoms has a substituent, the substituent is not particularly limited, and examples thereof include: alkyl groups having 1 to 30 carbon atoms, such as methyl, ethyl, propyl, isopropyl, and butyl; alkoxy groups having 1 to 30 carbon atoms, such as methoxy, ethoxy, and propoxy; hydroxyl groups; cyano groups; nitro groups; halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms), etc. The number of substituents may be one, or a combination of two or more substituents may be provided.

[0046] Furthermore, "these salts" refer to salts having a structure in which at least one of the hydroxyl groups in formulae (1) to (3) is converted into a hydroxide ion. Specifically, the salts include compounds represented by the following formulae (1-1) to (3-1).

[0047]

[0048] In the above formulas (1-1) to (3-1), R is the same as in formulas (1) to (3). + Each of the compounds of formula (1-1) to (3-1) may be a monovalent cation. + The compounds of formula (1-2) and (2-2) have two X in the compound + , may be a single divalent cation. For example, two compounds of formula (1-1) may have the following structures including a divalent cation.

[0049]

[0050] The monovalent cation is not particularly limited, and examples thereof include sodium cation, potassium cation, ammonium cation, quaternary ammonium cation (methylammonium cation, ethylammonium cation, dimethylammonium cation, trimethylammonium cation, tetramethylammonium cation), etc. These monovalent cations may be contained alone or in combination of two or more.

[0051] The divalent cation is not particularly limited, and examples thereof include a magnesium cation, a calcium cation, a strontium cation, and a barium cation.

[0052] Specific examples of the copper surface protective agent are not particularly limited, and include: compounds represented by formula (1) such as propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, nonylphosphonic acid, decylphosphonic acid, undecylphosphonic acid, dodecylphosphonic acid, phenylphosphonic acid, 4-methylphenylphosphonic acid, and naphthylphosphonic acid; compounds represented by formula (2) such as propyl phosphate, butyl phosphate, pentyl phosphate, hexyl phosphate, heptyl phosphate, octyl phosphate, nonyl phosphate, decyl phosphate, undecyl phosphate, dodecyl phosphate, phenyl phosphate, and 4-nitrophenyl phosphate; compounds represented by formula (3) such as propylbenzenesulfonic acid, butylbenzenesulfonic acid, pentylbenzenesulfonic acid, hexylbenzenesulfonic acid, heptylbenzenesulfonic acid, octylbenzenesulfonic acid, nonylbenzenesulfonic acid, decylbenzenesulfonic acid, undecylbenzenesulfonic acid, dodecylbenzenesulfonic acid, phenylbenzenesulfonic acid, and 4-dodecylbenzenesulfonic acid; and salts thereof. Among these, the copper surface protective agent preferably comprises at least one of the compounds represented by formula (1) and their salts, more preferably comprises at least one selected from the group consisting of propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, nonylphosphonic acid, decylphosphonic acid, undecylphosphonic acid, dodecylphosphonic acid and their salts, further preferably comprises at least one selected from the group consisting of heptylphosphonic acid, octylphosphonic acid, nonylphosphonic acid and their salts, particularly preferably comprises octylphosphonic acid and / or its salt. It should be noted that the above copper surface protective agent can be used alone or in combination of two or more.

[0053] Relative to the total mass of the copper surface protection composition, the content of the copper surface protection agent is preferably 0.00001 to 1 mass%, more preferably 0.0001 to 1 mass%, further preferably 0.001 to 0.5 mass%, and particularly preferably 0.005 to 0.1 mass%. If the content of the copper surface protection agent is 0.00001 mass% or more, a dense copper surface protection layer can be formed, so it is preferred. On the other hand, if the content of the copper surface protection agent is 1 mass% or less, it is easy to prepare a uniform composition, so it is preferred.

[0054] [Solvent]

[0055] The solvent is not particularly limited, and examples thereof include water and organic solvents.

[0056] The water is not particularly limited, but is preferably water from which metal ions, organic impurities, particles, and the like have been removed by distillation, ion exchange treatment, filtration treatment, various adsorption treatments, and the like. Pure water is more preferred, and ultrapure water is particularly preferred.

[0057] The organic solvent is not particularly limited, and examples thereof include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and tert-butanol; polyols such as ethylene glycol, propylene glycol, neopentyl glycol, 1,2-hexanediol, 1,6-hexanediol, 2-ethylhexane-1,3-diol, and glycerol; and glycol ethers such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol monoethyl ether, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether, tripropylene glycol n-propyl ether, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, and propylene glycol phenyl ether.

[0058] Among the above, the solvent is more preferably water. The above solvents may be used alone or in combination of two or more.

[0059] The addition rate of the solvent, especially water, is preferably 50 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and particularly preferably 95 mass % or more, based on the total mass of the copper surface protective composition.

[0060] [pH adjuster]

[0061] The pH adjuster has a function of adjusting the pH of the copper surface protective composition.

[0062] Examples of the pH adjuster include acidic compounds and basic compounds.

[0063] The acidic compound is not particularly limited, and examples thereof include inorganic strong acid compounds such as hydrogen chloride, hydrogen bromide, hydrogen iodide, sulfuric acid, and nitric acid; organic strong acid compounds such as methanesulfonic acid and benzenesulfonic acid; inorganic weak acid compounds such as phosphoric acid; and organic weak acid compounds such as acetic acid and citric acid.

[0064] The aforementioned alkaline compound is not particularly limited, and examples thereof include: inorganic strong base compounds such as sodium hydroxide, potassium hydroxide, calcium hydroxide, and barium hydroxide; organic strong base compounds such as tetramethylammonium hydroxide (TMAH) and tetraethylammonium hydroxide (TEAH); inorganic weak base compounds such as sodium carbonate and ammonia; organic weak base compounds such as diazabicycloundecene (DBU) and diazabicyclononene (DBU), etc.

[0065] Among these, the pH adjusting agent preferably includes at least one selected from the group consisting of an inorganic strong acid compound, an inorganic strong base compound and an inorganic weak base compound, more preferably includes at least one selected from the group consisting of sulfuric acid, nitric acid, sodium hydroxide, potassium hydroxide, calcium hydroxide, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH) and ammonia, further preferably includes at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, calcium hydroxide, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH) and ammonia, and particularly preferably includes at least one selected from the group consisting of sodium hydroxide, potassium hydroxide and calcium hydroxide. In addition, the above-mentioned pH adjusting agent can be used alone or in combination with two or more.

[0066] The content of the pH adjuster is not particularly limited, but is preferably an amount that allows the pH of the copper surface protective composition to be a desired pH.

[0067] [Physical properties of copper surface protective composition]

[0068] The pH of the copper surface protective composition is preferably 0.1 to 13, more preferably 1 to 12.5, further preferably 2 to 12, and further preferably 2.5 to 5.5. By adjusting the pH of the copper surface protective composition, a suitable copper surface protective layer can be formed on the copper surface. Although the reason for obtaining such an effect is not clear, for example, the change in the surface potential (zeta potential) of copper based on pH can be cited. Specifically, if the pH of the copper surface protective composition is acidic (pH is less than 7.0), there is a tendency for the copper surface to have more positive charges, and if the pH is alkaline (pH is greater than 7.0), there is a tendency for the copper surface to have more negative charges. It is believed that through such changes in the surface potential (zeta potential) of copper, the copper surface protective agent contained in the copper surface protective composition can interact with the copper surface appropriately.

[0069] <Method for producing semiconductor intermediate>

[0070] According to one embodiment of the present invention, a method for manufacturing a semiconductor intermediate can be provided. In this case, the semiconductor intermediate (first semiconductor intermediate) includes a copper-containing layer and a copper surface protection layer stacked on the aforementioned copper-containing layer. In addition, the method for manufacturing the aforementioned semiconductor intermediate includes the following step (1): on the aforementioned copper-containing layer in the first semiconductor having the copper-containing layer, the aforementioned copper surface protection composition is brought into contact to form a copper surface protection layer. In addition, for the intermediate of the aforementioned semiconductor, a step (cleaning step) of cleaning the aforementioned copper-containing layer using a cleaning solution before the aforementioned step (1) may also be included. Below, the cleaning step and step (1) are described in sequence. It should be noted that in this specification, "copper-containing layer" refers to a layer in which copper as a metal is at least present on the surface of the layer, and the copper-containing layer is preferably a layer composed of copper.

[0071] [Cleaning process]

[0072] The cleaning step is performed before step (1). The cleaning step is a step of cleaning the copper-containing layer in the first semiconductor having the copper-containing layer using a cleaning liquid.

[0073] (First Semiconductor)

[0074] The first semiconductor includes a copper-containing layer. The first semiconductor is not particularly limited, and examples thereof include a semiconductor chip or a semiconductor wafer.

[0075] (Cleaning fluid)

[0076] The cleaning liquid has a function of cleaning the surface of the copper-containing layer, for example, a function of removing copper oxide formed on the exposed surface of the copper-containing layer.

[0077] Cleaning fluids contain detergents and solvents.

[0078] The cleaning agent is not particularly limited, and includes at least one selected from the group consisting of acids and bases.

[0079] The acid is not particularly limited, and examples thereof include inorganic acids such as hydrofluoric acid, hydrogen chloride, hydrogen bromide, hydrogen iodide, sulfuric acid, nitric acid, and phosphoric acid; and organic acids such as acetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and 10-camphorsulfonic acid.

[0080] The base is not particularly limited, and examples thereof include ammonia and ammonium salts.

[0081] The ammonium salt is not particularly limited, and examples thereof include ammonium fluoride (NH4F); ammonium bifluoride (NH4F·HF); tetraalkylammonium hydroxides such as tetraethylammonium hydroxide (TEAH), tetramethylammonium hydroxide (TMAH), ethyltrimethylammonium hydroxide, diethyldimethylammonium hydroxide, triethylmethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide; aromatic group-containing ammonium hydroxides such as benzyltrimethylammonium hydroxide and benzyltriethylammonium hydroxide; hydroxyl group-containing ammonium hydroxides such as trimethyl(2-hydroxyethyl)ammonium hydroxide, triethyl(2-hydroxyethyl)ammonium hydroxide, tripropyl(2-hydroxyethyl)ammonium hydroxide, and trimethyl(1-hydroxypropyl)ammonium hydroxide; and the like.

[0082] Among them, the cleaning agent preferably contains at least one selected from the group consisting of acid and ammonia, more preferably contains at least one selected from the group consisting of hydrofluoric acid, hydrogen chloride, hydrogen bromide, hydrogen iodide, sulfuric acid, nitric acid and ammonia, further preferably contains at least one selected from the group consisting of hydrofluoric acid, sulfuric acid, nitric acid and ammonia, particularly preferably contains at least one selected from the group consisting of sulfuric acid, nitric acid and ammonia, and most preferably contains sulfuric acid. In addition, the cleaning agent can be used alone or in combination of two or more.

[0083] The content of the cleaning agent is preferably 0.001 to 50 mass %, more preferably 0.01 to 10 mass %, further preferably 0.03 to 3 mass %, particularly preferably 0.05 to 2 mass %, relative to the total mass of the cleaning liquid.

[0084] The aforementioned solvent is not particularly limited, and may be the same as the solvent used in the copper surface protection composition. Among them, the solvent is preferably water. In addition, the aforementioned solvent may be used alone or in combination of two or more.

[0085] The addition ratio of the solvent, especially water, is preferably 50 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and particularly preferably 95 mass % or more, based on the total mass of the cleaning liquid.

[0086] The cleaning solution may further contain a pH adjusting agent. The pH adjusting agent is not particularly limited, and examples thereof include the same pH adjusting agents as those used in the copper surface protective composition. These pH adjusting agents may be used alone or in combination of two or more.

[0087] The pH of the washing liquid is not particularly limited, but is preferably 0.1 to 13, more preferably 0.5 to 10, further preferably 0.5 to 5, and particularly preferably 0.4 to 2.5.

[0088] (Cleaning)

[0089] The cleaning method is not particularly limited, and known techniques can be appropriately used. Specifically, the first semiconductor can be immersed in the cleaning solution, or the cleaning solution can be sprayed on the surface of the copper-containing layer of the first semiconductor, or it can be dripped (single-wafer rotation treatment). At this time, the aforementioned dipping can be repeated more than 2 times, the spraying can be repeated more than 2 times, the dripping can be repeated more than 2 times, and the dipping, spraying and dripping can be combined.

[0090] The washing temperature is not particularly limited, but is preferably 0 to 90°C, more preferably 5 to 70°C, and further preferably 10 to 50°C.

[0091] The washing time is not particularly limited, but is preferably 10 seconds to 3 hours, more preferably 10 seconds to 1 hour, further preferably 15 seconds to 45 minutes, and particularly preferably 30 seconds to 20 minutes.

[0092] [Process (1)]

[0093] Step (1) is a step of bringing the copper surface protective composition into contact with the copper-containing layer in the first semiconductor having the copper-containing layer to form a copper surface protective layer.

[0094] (First Semiconductor)

[0095] The above-mentioned semiconductor is used as the first semiconductor. At this time, the first semiconductor is preferably subjected to the above-mentioned cleaning step to remove copper oxide that the copper-containing layer may have.

[0096] (Copper surface protective composition)

[0097] The copper surface protective composition used is the copper surface protective composition described above.

[0098] (touch)

[0099] The contact method is not particularly limited, and known techniques can be appropriately used. Specifically, the first semiconductor can be immersed in the copper surface protective composition, the copper surface protective composition can be sprayed on the surface of the copper-containing layer of the first semiconductor, or it can be added dropwise (single-wafer rotation treatment, etc.). At this time, the aforementioned immersion can be repeated more than 2 times, the spraying can be repeated more than 2 times, the dropping can be repeated more than 2 times, and the immersion, spraying and dropping can be combined.

[0100] The contact temperature is not particularly limited, but is preferably 0 to 90°C, more preferably 5 to 70°C, and further preferably 10 to 65°C.

[0101] The contact time is not particularly limited, but is preferably 10 seconds to 3 hours, more preferably 10 seconds to 1 hour, further preferably 1 to 45 minutes, and particularly preferably 3 to 20 minutes.

[0102] After the contact, the excess copper surface protective composition is washed off with water, isopropyl alcohol or the like as appropriate to remove the solvent contained in the copper surface protective composition adhering to the surface of the copper-containing layer, thereby forming a copper surface protective layer.

[0103] [Copper surface protective layer]

[0104] The copper surface protective layer contains a copper surface protective agent. Since the copper surface protective layer is a dense layer, oxygen is not easy to penetrate. As a result, oxygen can be prevented from contacting the copper-containing layer, and oxidation of the surface of the copper-containing layer can be prevented.

[0105] The thickness of the copper surface protective layer is not particularly limited, and is preferably 0.1 to 50 nm, more preferably 0.2 to 10 nm, further preferably 0.3 to 2 nm, and particularly preferably 0.4 to 1 nm. It should be noted that in this specification, the thickness of the "copper surface protective layer" refers to the maximum thickness of the copper surface protective layer in the vertical direction relative to the contact surface of the copper-containing layer and the copper surface protective layer.

[0106] [First Semiconductor Intermediate]

[0107] The first semiconductor intermediate includes a copper-containing layer and a copper surface protection layer stacked on the copper-containing layer. In addition, depending on the structure of the first semiconductor, the copper surface protection layer may cover a portion or all of other layers such as an insulating layer and a silicon substrate layer in addition to the copper-containing layer.

[0108] In the first semiconductor intermediate, since the copper surface protection layer is formed on the copper-containing layer, oxidation of the surface of the copper-containing layer can be prevented. Therefore, the first semiconductor intermediate can be stored for a long time.

[0109] <Method for manufacturing semiconductor>

[0110] According to one embodiment of the present invention, a method for manufacturing a semiconductor is provided. In this case, the semiconductor includes a copper-containing bonding layer. In addition, the method for manufacturing the semiconductor includes: a step of removing the copper surface protection layer of the first semiconductor intermediate manufactured by the above method to expose the copper-containing layer (exposure step); and a step of bonding the exposed copper-containing layer with the metal-containing layer in the second semiconductor intermediate including the metal-containing layer to form a copper-containing bonding layer (bonding step). It should be noted that in this specification, "metal-containing layer" refers to a layer in which at least metal exists on the surface of the layer, and the metal-containing layer is preferably a layer composed of metal. In this case, the "metal" is capable of bonding with copper, preferably copper, tin, and more preferably copper.

[0111] [Exposure process]

[0112] The exposing step is a step of removing the copper surface protection layer of the first semiconductor intermediate to expose the copper-containing layer.

[0113] (First Semiconductor Intermediate)

[0114] As the first semiconductor intermediate, the above-mentioned first semiconductor intermediate is used.

[0115] (removed)

[0116] The method for removing the copper surface protective layer of the first semiconductor intermediate is not particularly limited, but preferably heating, hydrogen ashing, or ion irradiation of an inert gas is used, and more preferably heating is used. In addition, heating can also be performed under an inert gas atmosphere. Examples of inert gases include nitrogen and argon.

[0117] The heating temperature is not particularly limited, but is preferably 100 to 300°C, more preferably 150 to 250°C.

[0118] The heating time is not particularly limited, but is preferably 0.1 second to 3 hours, more preferably 1 second to 1 hour, further preferably 10 seconds to 15 minutes, and particularly preferably 1 minute to 15 minutes.

[0119] By removing the copper surface protection layer of the first semiconductor, the copper-containing layer can be exposed. That is, the first semiconductor having the copper-containing layer can be obtained.

[0120] [Joining process]

[0121] The bonding step is a step of bonding the exposed copper-containing layer to the metal-containing layer in the second semiconductor intermediate including the metal-containing layer to form a copper-containing bonding layer.

[0122] (Exposed copper layer)

[0123] Since the exposed copper-containing layer is covered with the copper surface protection layer before the exposure step and is hardly exposed to oxygen, the copper on the surface of the exposed copper-containing layer is hardly oxidized.

[0124] (Second Semiconductor Intermediate Comprising a Metal-Containing Layer)

[0125] The second semiconductor intermediate includes a metal-containing layer. The second semiconductor intermediate is not particularly limited, and a semiconductor chip or a semiconductor wafer may be cited. It should be noted that when the metal-containing layer is a copper-containing layer, the second semiconductor intermediate may also be manufactured in the same manner as the first semiconductor intermediate. In this case, the second semiconductor intermediate is used in the bonding process after the above-mentioned exposure process.

[0126] (engagement)

[0127] By bonding, the copper-containing layer and the metal-containing layer are connected to each other, and a three-dimensional (3D) integrated semiconductor can be obtained.

[0128] The bonding method is not particularly limited, but thermal compression bonding is preferred.

[0129] The bonding temperature is not particularly limited, but is preferably 80 to 500°C, more preferably 90 to 300°C, further preferably 100 to 250°C, and particularly preferably 120 to 200°C.

[0130] The bonding time is not particularly limited, but is preferably 0.01 to 600 seconds, more preferably 0.1 to 60 seconds.

[0131] Example

[0132] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0133] [Example 1]

[0134] A copper surface protective composition was prepared by mixing butylphosphonic acid as a copper surface protective agent and water as a solvent. At this time, the content of butylphosphonic acid was 0.01% by mass relative to the total mass of the copper surface protective composition.

[0135] The pH of the copper surface protective composition was measured and found to be 3.2. The pH was measured at 23°C using a tabletop pH meter (F-71) (manufactured by HORIBA, Ltd.) and a pH electrode (9615S-10D) (manufactured by HORIBA, Ltd.).

[0136] [Example 2]

[0137] A copper surface protective composition was prepared in the same manner as in Example 1 except that hexylphosphonic acid was used as the copper surface protective agent. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 3.3.

[0138] [Example 3]

[0139] A copper surface protective composition was prepared in the same manner as in Example 1 except that octylphosphonic acid was used as the copper surface protective agent. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 3.4.

[0140] [Example 4]

[0141] A copper surface protective composition was prepared in the same manner as in Example 1 except that dodecyl phosphate was used as a copper surface protective agent in an amount of 0.001 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 4.5.

[0142] [Example 5]

[0143] A copper surface protective composition was prepared in the same manner as in Example 1 except that phenylphosphonic acid was used as the copper surface protective agent. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was found to be 3.2.

[0144] [Example 6]

[0145] A copper surface protective composition was prepared in the same manner as in Example 1 except that 4-dodecylbenzenesulfonic acid was used as a copper surface protective agent in an amount of 0.05 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 2.9.

[0146] [Example 7]

[0147] A copper surface protective composition was prepared in the same manner as in Example 3 except that sulfuric acid was further added as a pH adjuster so as to have a content of 1 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 1.2.

[0148] [Example 8]

[0149] A copper surface protective composition was prepared in the same manner as in Example 3 except that sulfuric acid was further added as a pH adjuster in an amount of 0.05 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 2.1.

[0150] [Example 9]

[0151] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.0006 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 4.0.

[0152] [Example 10]

[0153] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.0007 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 5.0.

[0154] [Example 11]

[0155] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.0012 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 6.0.

[0156] [Example 12]

[0157] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.0014 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 7.0.

[0158] [Example 13]

[0159] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.0016 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 8.0.

[0160] [Example 14]

[0161] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.0031 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 9.0.

[0162] [Example 15]

[0163] A copper surface protective composition was produced in the same manner as in Example 3 except that ammonia was further added as a pH adjuster so as to have a content of 0.013 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 10.0.

[0164] [Example 16]

[0165] A copper surface protective composition was prepared in the same manner as in Example 3 except that tetramethylammonium hydroxide (TMAH) was further added as a pH adjuster to a content of 0.018 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 11.0.

[0166] [Example 17]

[0167] A copper surface protective composition was prepared in the same manner as in Example 3 except that tetramethylammonium hydroxide (TMAH) was further added as a pH adjuster to a content of 0.075 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 12.0.

[0168] [Example 18]

[0169] A copper surface protective composition was prepared in the same manner as in Example 3 except that sodium hydroxide (NaOH) was further added as a pH adjuster so as to have a content of 0.0026 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 5.0.

[0170] [Example 19]

[0171] A copper surface protective composition was prepared in the same manner as in Example 3 except that potassium hydroxide (KOH) was further added as a pH adjuster so as to have a content of 0.0029 mass %. The pH of the copper surface protective composition was measured in the same manner as in Example 1 and was 5.0.

[0172] [Comparative Example 1]

[0173] A composition was prepared in the same manner as in Example 1 except that benzotriazole was used in an amount of 0.05 mass % instead of the copper surface protective agent. The pH of the composition was measured in the same manner as in Example 1 and was 5.2.

[0174] [Comparative Example 2]

[0175] A composition was prepared in the same manner as in Example 1 except that dodecylpyridinium chloride was used in place of the copper surface protective agent so as to have a content of 0.05 mass %. The pH of the composition was measured in the same manner as in Example 1 and was 4.7.

[0176] [Comparative Example 3]

[0177] A composition was prepared in the same manner as in Example 1 except that 1-hydroxyethane-1,1-diphosphonic acid was used in place of the copper surface protective agent so as to have a content of 0.5 mass %. The pH of the composition was measured in the same manner as in Example 1 and was 1.7.

[0178] [Comparative Example 4]

[0179] A composition was prepared in the same manner as in Example 1 except that poly(ammonium 4-styrenesulfonate) (weight average molecular weight Mw=200,000) was used in place of the copper surface protective agent to give a content of 0.05 mass %. The pH of the composition was measured in the same manner as in Example 1 and was 4.8.

[0180] The copper surface protective compositions and the like produced in Examples 1 to 19 and Comparative Examples 1 to 4 are shown in Table 1 below.

[0181] [Table 1]

[0182]

[0183] In addition, the structural formula of the copper surface protective agent etc. used in Examples and Comparative Examples is as follows.

[0184]

[0185] [evaluate]

[0186] Various evaluations were performed on the copper surface protective compositions and the like produced in Examples 1 to 19 and Comparative Examples 1 to 4.

[0187] (Copper oxidation rate)

[0188] (1) Preparation of Cu-plated samples

[0189] SiO2 (thickness: )、TaN(Thickness: )、Ta(Thickness: )、seed Cu(thickness: )、Cu plating (thickness: ) of the Cu-plated samples.

[0190] (2) Pre-treatment

[0191] 1cm×1cm (immersion treatment area: 1cm 2 The Cu-plated sample was immersed in 10 mL of 1% hydrofluoric acid (DHF) at 23° C. for 1 minute to remove copper oxide (CuO) on the surface of the Cu-plated sample. Then, it was rinsed with water at 23° C. for 10 seconds and purged with nitrogen to remove water from the surface.

[0192] (3) Formation of copper surface protective layer

[0193] The Cu-plated sample after removal of copper oxide was immersed in a copper surface protective composition at 20° C. for 10 minutes. Then, water was rinsed at 23° C. for 10 seconds and nitrogen was purged to remove water from the surface and form a copper surface protective layer on the Cu-plated sample.

[0194] (4) Evaluation of copper oxidation rate

[0195] The Cu-plated samples on which the copper surface protective layer was formed were stored in the atmosphere at 20° C. for 24 hours or 120 hours.

[0196] The copper oxidation rate in the stored Cu-plated sample with a copper surface protective layer was determined. Specifically, the stored Cu-plated sample with a copper surface protective layer was analyzed by X-ray photoelectron spectroscopy (XPS; PHI Quantera II manufactured by ULVAC-PHI, INCORPORATED) to obtain a narrow scan spectrum of Cu2p. The obtained narrow scan spectrum of Cu2p was analyzed by curve fitting to calculate Cu 2+ Individual peak areas, and Cu + The peak area obtained is used to calculate the copper oxidation rate (using Cu 2+ The peak area of ​​Cu + It should be noted that the higher the copper oxidation rate, the higher the peak area of ​​Cu + Compared with Cu, Cu 2+ The more, the more the Cu-plated surface of the Cu sample is oxidized during the storage period of the Cu-plated sample. The obtained results are shown in Table 2 below. It should be noted that Table 2 also shows the results of the reference example in which "(3) formation of a copper surface protective layer" (no copper surface protective composition, etc.) is performed.

[0197] (Removability of copper surface protective layer)

[0198] (1) Preparation and pretreatment of Cu samples

[0199] In the same manner as in the above-mentioned evaluation of copper oxidation rate, a pre-treated Cu-plated sample was prepared.

[0200] (2) Formation of copper surface protective layer

[0201] The Cu-plated sample after removing the copper oxide is immersed in a copper surface protective composition at 20°C for 10 minutes. Then, water is rinsed at 23°C for 10 seconds and nitrogen is purged to remove water from the surface to obtain a Cu-plated sample with a copper surface protective layer. It should be noted that the contact angle of water on the surface of the Cu-plated sample with a copper surface protective layer is measured, and the result is more than 60 degrees. Since the copper surface protective layer is an organic layer, there is a tendency for the contact angle of water to increase compared to the copper surface with high surface free energy.

[0202] (3) Evaluation of the removability of the copper surface protective layer

[0203] The Cu sample with the copper surface protective layer formed thereon was placed on a hot plate heated to 200° C. for 5 minutes to remove the copper surface protective layer.

[0204] The contact angle of water on the surface of the Cu sample before and after the hot plate was left still was measured and evaluated according to the following benchmark. In addition, if the copper surface protective layer is removed by heating, the copper surface with high surface free energy will be exposed, thereby there is a tendency for the contact angle to decrease. The results obtained are shown in Table 2 below.

[0205] ○: Water contact angle is less than 25 degrees

[0206] ×: The contact angle of water is 25 degrees or more

[0207] [Table 2]

[0208]

[0209] *ND: No data

[0210] From the results in Table 2, it is understood that the copper surface protective compositions of Examples 1 to 19 can suitably prevent oxidation of the copper surface by protecting the copper surface.

[0211] [Influence of pretreatment agents]

[0212] The influence of the pretreatment agent on the copper surface before the copper surface protection layer is formed from the copper surface protection composition was evaluated.

[0213] (1) 1% hydrofluoric acid (DHF)

[0214] The copper oxidation rate and removability were evaluated in the same manner as above using the copper surface protective composition of Example 3. This example uses 1% hydrofluoric acid (DHF) as a pretreatment agent.

[0215] (2) 1% sulfuric acid

[0216] The copper oxidation rate and removability were evaluated in the same manner as in the above (1) except that 1% sulfuric acid was used as the pretreatment agent.

[0217] (3) 0.1% ammonia

[0218] The copper oxidation rate and removability were evaluated in the same manner as in the above (1) except that 0.1% ammonia was used as the pretreatment agent.

[0219] The results obtained in the above (1) to (3) are shown in Table 3 below.

[0220] [Table 3]

[0221]

[0222] *ND: No data

[0223] From the results in Table 3, it is understood that even when any pretreatment agent is used, oxidation of the copper surface can be suitably prevented by protecting the copper surface.

Claims

1. A copper surface protective composition comprising a copper surface protective agent and a solvent, The copper surface protective agent is at least one selected from the group consisting of compounds represented by the following formulas (1) to (3) and their salts, In the formulae (1) to (3), R is a substituted or unsubstituted alkyl group having 3 to 30 carbon atoms or a substituted or unsubstituted aryl group having 6 to 30 carbon atoms.

2. The copper surface protective composition according to claim 1, wherein The copper surface protective agent comprises the compound represented by formula (1) and / or its salt.

3. The copper surface protective composition according to claim 1 or 2, wherein The R is a substituted or unsubstituted alkyl group having 3 to 30 carbon atoms. 4 . The copper surface protective composition according to claim 1 , further comprising a pH adjuster.

5. The copper surface protective composition according to claim 4, wherein The pH adjuster includes at least one selected from the group consisting of sodium hydroxide and potassium hydroxide. 6 . The copper surface protective composition according to claim 1 , wherein the pH thereof is 2.5 to 5.

5. 7 . The copper surface protective composition according to claim 1 , which is used for production of a semiconductor.

8. A method for producing a first semiconductor intermediate, comprising a copper-containing layer and a copper surface protection layer stacked on the copper-containing layer, the method comprising the following step (1): The copper surface protective layer is formed by bringing the copper surface protective composition according to any one of claims 1 to 7 into contact with the copper-containing layer in the first semiconductor having the copper-containing layer.

9. The method for manufacturing a first semiconductor intermediate according to claim 8, comprising: Before the step (1), a step of cleaning the copper-containing layer using a cleaning solution is performed.

10. The method for manufacturing a first semiconductor intermediate according to claim 9, wherein: The cleaning solution includes at least one selected from the group consisting of hydrofluoric acid, sulfuric acid, nitric acid, and ammonia.

11. A method for manufacturing a semiconductor, which is a method for manufacturing a semiconductor including a copper-containing bonding layer, the manufacturing method comprising: A step of removing the copper surface protection layer of the first semiconductor intermediate produced by the method according to any one of claims 8 to 10 to expose the copper-containing layer; and The step of bonding the exposed copper-containing layer to the metal-containing layer in the second semiconductor intermediate including the metal-containing layer to form a copper-containing bonding layer.