Pot easy to clean and manufacturing method thereof
By forming concave and convex patterns on the inner surface of the pot and forming a metal layer using physical vapor deposition technology, the problems of poor non-stickness of the pot and food hygiene and safety are solved, and efficient cleaning and long life of the pot are achieved.
Patent Information
- Application Number
- CN202310527159.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
AI Technical Summary
During use, existing pots and utensils are prone to fall off due to the non-stick coating, which makes it difficult to stick to the pot and clean the ingredients, and the exposure of the substrate to a high-temperature and high-humidity environment poses food hygiene and safety risks.
The metal layer is formed on the inner surface of the pot, and a metal layer is formed through physical vapor deposition technology. The metal layer is composed of metal particles and metal nitride particles. The metal nitride particles are filled in the gap micropores of the metal particles, and the thickness of the metal layer is The nitride content is controlled at 0.5-1.5 μm and 20-35 wt% to improve non-stickness and wear resistance.
It effectively avoids cracking of metal layers, improves the non-stickness, wear resistance and food hygiene and safety of the pot, extends the service life, and improves user experience and cleaning convenience.
Smart Images

Figure CN118902276A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cookware, and in particular to an easy-to-clean cookware and a manufacturing method thereof. Background Art
[0002] In order to achieve the non-stick effect of food, existing cookware usually applies a non-stick coating on the inner surface of the cookware. However, this non-stick coating is easy to fall off due to scratches or hot and cold shocks during use and has a limited service life, so it is impossible to achieve a long-term non-stick effect of the cookware. In addition, the detached coating will be mixed with the food and accidentally eaten, affecting human health. At the same time, after the coating falls off, the base material of the cookware is directly exposed to a high temperature and high humidity environment during the cooking process, and there is a risk of heavy metals in the base material precipitating into the food, which poses a food hygiene and safety problem and makes the cookware unsuitable for continued use. In order to solve the above problems, uncoated cookware is made, such as using a stainless steel or titanium layer on the inner surface of the cookware, but it is easy for the food to stick to the pot and is difficult to clean, which reduces the user experience. Summary of the invention
[0003] In order to solve the above-mentioned shortcomings and deficiencies in the prior art, the present invention provides an easy-to-clean cookware to solve the technical problem of poor non-stick effect of cookware without coating, thereby improving the user experience.
[0004] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:
[0005] One aspect of the present invention provides an easy-to-clean cookware, comprising:
[0006] A pot body, wherein the inner surface of the pot body is formed with concave-convex patterns;
[0007] The metal layer is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles are at least partially filled in the gap micropores of the metal particles.
[0008] Optionally, the metal particles are deposited to form a metal film, and the metal film covers the surface of the film formed by the deposition of metal nitride particles.
[0009] Optionally, the thickness of the metal layer is 0.5-1.5 μm.
[0010] Optionally, the content of metal nitride in the metal layer is 20-35 wt %. Optionally, the thickness of the metal layer in the area of the pot body flange is not less than the thickness of the metal layer in the area of the pot body bottom wall.
[0011] Optionally, the concave-convex pattern includes concave portions and convex ridges formed between two adjacent concave portions, and the concave portions are distributed in a lattice shape on the inner surface of the pot body.
[0012] Another aspect of the present invention provides a method for manufacturing the easy-to-clean cookware as described in any one of the above items, comprising the following steps:
[0013] S1: etching or mechanically punching the metal sheet so that a concave-convex pattern is formed on one side of the surface of the metal sheet;
[0014] S2: stretching the metal sheet into a pot body so that the concave and convex patterns are located on the inner surface of the pot body;
[0015] S3: Performing physical vapor deposition on the inner surface of the pot body to form a metal layer, wherein the metal layer is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles at least partially fill the gap micropores of the metal particles.
[0016] Optionally, the method of the physical vapor deposition treatment is: using a target material to deposit a metal layer on the inner surface of the pot body according to preset deposition parameters.
[0017] Optionally, the preset deposition parameters include: deposition gas pressure, deposition gas flow rate, deposition power and deposition time, wherein the deposition gas pressure is 2 to 4×10-2 Torr, the deposition gas flow rate is 200 to 500 sccm, the deposition power is 5 to 8 kW, and the deposition time is 10 to 20 min.
[0018] Optionally, before step S3, the inner surface of the pot body is pre-plasma cleaned.
[0019] Compared with the prior art, the beneficial effects of the present invention include but are not limited to:
[0020] 1. The present invention forms a concave-convex pattern on the inner surface of the pot body, so that the inner surface of the pot body becomes a rough surface with a certain roughness. A metal layer with a concave-convex structure identical to the concave-convex pattern is formed on the rough surface by physical vapor deposition, which not only improves the bonding force between the metal layer and the pot body, but also greatly eliminates the intrinsic stress of the metal layer, and also improves the density of the metal layer, effectively avoiding the problem of cracking of the metal layer during the use of the pot. At the same time, the concave-convex structure of the metal layer makes the surface of the metal layer also form a rough surface with a certain roughness, and the concave part of the concave-convex structure is filled with air, which reduces the surface energy of the metal layer, improves the hydrophobicity of the metal layer, and improves the non-stick effect. Furthermore, the metal layer is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles are at least partially filled in the gap micropores of the metal particles. Due to the filling of the metal nitride particles, the hardness of the metal layer is further improved and the surface energy of the metal layer is reduced, which effectively improves the wear resistance and non-stickiness of the pot, makes the pot easy to clean and has a long service life, and improves the user experience.
[0021] 2. The present invention forms a metal film by depositing metal particles, and the metal film covers the surface of the film formed by the deposition of metal nitride particles. In this way, the hardness of the film formed by the deposition of metal nitride particles is greater than the hardness of the metal film formed by the deposition of metal particles, which can play a certain supporting role on the metal film, improve the hardness of the metal film, and improve the wear resistance of the metal film. Especially after the metal film is worn, the film formed by the deposition of metal nitride can continue to cover the pot body, avoiding the pot body from being directly exposed to a high temperature and high humidity environment, thereby ensuring the food hygiene and non-stickiness of the cookware, extending the service life of the cookware and facilitating cleaning.
[0022] 3. The thickness of the metal layer of the present invention is 0.5-1.5 μm. This can not only prevent the pot body from being exposed due to incomplete coverage by the metal layer, but also make the metal layer have a certain hardness to ensure the non-stickiness, wear resistance and food hygiene safety of the pot, but also avoid the increase in the manufacturing cost of the pot due to the excessive thickness of the metal layer.
[0023] 4. The content of metal nitride in the metal layer of the present invention is 20-35wt%, which can not only ensure the hardness of the metal layer and improve the wear resistance of the metal layer, but also effectively reduce the surface energy of the metal layer, improve the non-stick property, and facilitate the cleaning of the pot.
[0024] 5. In cooking utensils such as rice cookers, pressure cookers and frying pans, the flange area of the pot is in frequent contact with the lid body. Long-term use will cause the surface of the flange area to wear. The worn flange area is exposed to a high temperature and high humidity environment, and there is a risk of heavy metals in the pot base material precipitating into the food. By ensuring that the thickness of the metal layer in the area of the pot flange is not less than the thickness of the metal layer in the area of the pot bottom wall, the wear resistance of the metal layer in the area of the pot flange is improved, the food hygiene and safety of the cookware is guaranteed, and the service life of the cookware is extended.
[0025] 6. The concave-convex pattern in the present invention includes a concave portion and a convex ridge formed between two adjacent concave portions, and the concave portions are distributed in a dot matrix on the inner surface of the pot body. In this way, the concave-convex pattern is evenly distributed on the inner surface of the pot body, effectively reducing the surface energy of the inner surface of the pot, improving the non-stick property of the pot, and facilitating the cleaning of the pot. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0027] Figure 1 It is a schematic structural diagram of a pot body in one embodiment of the present invention;
[0028] Figure 2is a partial cross-sectional schematic diagram of a cooker in one embodiment of the present invention;
[0029] Figure 3 is a partial cross-sectional schematic diagram of a cooker in another embodiment of the present invention;
[0030] Reference numerals:
[0031] 100 pot body; 110 concave-convex pattern; 111 concave portion; 112 convex ridge; 113 pot body flange; 114 pot body bottom wall; 200 metal layer; 210 metal film; 220 film. DETAILED DESCRIPTION
[0032] In order to more clearly illustrate the overall concept of the present application, a detailed description is given below in an illustrative manner in conjunction with the accompanying drawings.
[0033] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application may also be implemented in other ways different from those described herein. Therefore, the scope of protection of the present application is not limited to the specific embodiments disclosed below.
[0035] In addition, in the description of the present application, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0036] In the present application, unless otherwise clearly specified and limited, a first feature "above" or "below" a second feature may be that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in an appropriate manner in any one or more embodiments or examples.
[0037] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0038] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0039] Example 1
[0040] Combination Figures 1 to 3 As shown, this embodiment provides an easy-to-clean cookware, including: a pot body 100, the inner surface of which is formed with a concave-convex pattern 110; a metal layer 200, which is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles are at least partially filled in the gap micropores of the metal particles.
[0041] Combination Figure 2 As shown, since the inner surface of the pot body 100 is formed with the concavo-convex pattern 110, the inner surface of the pot body 100 becomes a rough surface with a certain roughness, and a metal layer 200 having the same concavo-convex structure as the concavo-convex pattern 110 is formed on the rough surface by physical vapor deposition, which not only improves the bonding force between the metal layer 200 and the pot body 100, but also greatly eliminates the inherent stress of the metal layer 200, and also improves the density of the metal layer 200, effectively avoiding the problem of cracking of the metal layer 200 during the use of the pot, and at the same time, the concavo-convex structure of the metal layer 200 makes the surface of the metal layer A rough surface with a certain roughness is formed, and the concave parts of the concave-convex structure are filled with air, which reduces the surface energy of the metal layer 200, improves the hydrophobicity of the metal layer 200, and improves the non-stick effect; further, the metal layer 200 is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles are at least partially filled in the gap micropores of the metal particles. Due to the filling of the metal nitride particles, the hardness of the metal layer 200 is further improved and the surface energy of the metal layer is reduced, which effectively improves the wear resistance and non-stick properties of the pot, making the pot easy to clean and have a long service life, thereby improving the user experience. Figure 2As shown, the black area in the figure is the deposited metal nitride.
[0042] It should be noted that the above-mentioned “inner surface” refers to the surface of the pot body 100 close to the food when the pot is in use, that is, after the metal layer 200 is formed by physical vapor deposition, the metal layer 200 directly contacts the food.
[0043] In the embodiment of the present invention, the material forming the pot body 100 is selected from at least one of stainless steel, iron, aluminum alloy and carbon steel; preferably, the material of the pot body is stainless steel. The above materials have good thermal conductivity and can meet the use requirements of the pot.
[0044] It should be noted that the above-mentioned “metal particles” include at least one of metal ions, metal atoms, and metal molecules; the above-mentioned “metal nitride particles” include at least one of metal nitride ions, metal nitride atoms, and metal nitride molecules.
[0045] In the embodiment of the present invention, the “metal particles” include titanium particles or chromium particles, etc., and the “metal nitride particles” include titanium nitride particles or chromium nitride particles, etc.
[0046] It should be noted that the cookware in the present invention can be a wok, a frying pan, a scalding pot, or the inner liner of a rice cooker or a pressure cooker. For example, the inner surface of the stainless steel inner liner of a rice cooker or a pressure cooker is treated with physical vapor deposition to deposit a metal layer. It should be pointed out that the cookware in the present invention is not limited to the above-mentioned uses.
[0047] In an embodiment of the present invention, Figure 2 As shown, the concave-convex pattern 110 includes a concave portion 111 and a convex ridge 112 formed between two adjacent concave portions 111, and the concave portions 111 are distributed in a dot matrix on the inner surface of the pot body 100. In this way, the concave-convex pattern is evenly distributed on the inner surface of the pot body 100, effectively reducing the surface energy of the inner surface of the pot, improving the non-stick property of the pot, and facilitating the cleaning of the pot.
[0048] In an embodiment of the present invention, the thickness of the metal layer is 0.5-1.5 μm. In this way, it can not only avoid that the pot body 100 is not completely covered by the metal layer 200 and is exposed, but also make the metal layer 200 have a certain hardness, ensure the non-stickiness, wear resistance and food hygiene safety of the pot, and avoid the increase in the manufacturing cost of the pot due to the excessive thickness of the metal layer 200. Preferably, the lower limit of the thickness of the metal layer can be 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm or 1.4 μm; the upper limit of the thickness of the metal layer can be 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm or 1.4 μm.
[0049] In an embodiment of the present invention, the content of the metal nitride in the metal layer 200 is 20-35wt%, so that not only the hardness of the metal layer 200 can be ensured and the wear resistance of the metal layer 200 can be improved, but also the surface energy of the metal layer 200 can be reduced, the non-stickiness can be improved, and the cleaning of the pot is convenient. Preferably, the lower limit of the content of the metal nitride in the metal layer can be 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt% or 34wt%; the upper limit of the content of the metal nitride in the metal layer can be 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt% or 34wt%.
[0050] In another embodiment of the present invention, Figure 3 As shown, metal particles are deposited to form a metal film 210, and the metal film 210 covers the surface of a film 220 formed by the deposition of metal nitride particles. Since the hardness of the film 220 formed by the deposition of metal nitride is greater than that of the metal film 210 formed by the deposition of metal particles, it can play a certain supporting role for the metal film 210, improve the hardness of the metal film 210, and improve the wear resistance of the metal film 210. In particular, after the metal film 210 is worn, the film 220 formed by the deposition of metal nitride can continue to cover the pot body 100, preventing the pot body 100 from being directly exposed to a high temperature and high humidity environment, ensuring the food hygiene safety and non-stickiness of the pot, extending the service life of the pot and facilitating cleaning. Those skilled in the art may also understand that the inner surface of the pot body 100 is treated by physical vapor deposition to form a metal layer 200, wherein the metal layer 200 is composed of a film 220 and a metal film 210 from the inside to the outside, or the metal layer 200 is composed of a first metal film 210, a film 220 and a second metal film 210 from the inside to the outside, and the second metal film 210 is in direct contact with the food.
[0051] In another embodiment of the present invention, the thickness of the metal layer 200 at the pot flange 113 is not less than the thickness of the metal layer at the pot bottom wall 114 .
[0052] In cooking utensils such as rice cookers, pressure cookers and frying pans, the flange area of the cookware is in frequent contact with the cover body. Long-term use will cause the surface of the flange area to wear. The worn flange area is exposed to a high temperature and high humidity environment, and there is a risk of heavy metals in the base material of the cooker body being precipitated into the food. By ensuring that the thickness of the metal layer 200 in the area of the pot body flange 113 is not less than the thickness of the metal layer 200 in the area of the pot body bottom wall 114, the wear resistance of the metal layer 200 in the area of the pot body flange 113 is improved, the food hygiene and safety of the cookware is guaranteed, and the service life of the cookware is extended.
[0053] Example 2
[0054] This embodiment provides a method for manufacturing the cookware of the above-mentioned embodiment 1, which specifically comprises the following steps:
[0055] S1: Surface pretreatment of metal sheets;
[0056] Specifically, the metal sheet is etched or mechanically stamped so that a concave-convex pattern is formed on one side of the metal sheet. In actual production, etching or mechanical stamping process can be selected as needed. Compared with mechanical stamping, chemical etching is generally used. The concave-convex pattern formed by chemical etching is conducive to the adhesion of the metal layer to increase the bonding force with the metal layer, and is more uniform, with low cost and high production efficiency.
[0057] S2: Pot body forming;
[0058] The pot body can be formed by stretching, die casting, and forging. In actual production, it can be selected according to needs. Generally, stretching is used, which has low cost and higher production efficiency. Specifically, the metal sheet is stretched to form the pot body, so that the concave and convex patterns are located on the inner surface of the pot body.
[0059] S3: metal layer preparation;
[0060] The inner surface of the pot body is subjected to physical vapor deposition treatment to form a metal layer, which is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles at least partially fill the gap micropores of the metal particles.
[0061] Physical vapor deposition in the present invention refers to a technology that uses physical methods under vacuum conditions to vaporize the surface of a material into gaseous atoms or molecules, or partially ionize it into ions, and deposits a thin film with special functions on the surface of a substrate. The film has strong adhesion and high density.
[0062] Specifically, in order to form a stable metal layer with good hardness and wear resistance on the inner surface of the pot body using a target material through physical vapor deposition technology, the metal layer is deposited on the inner surface of the pot body using the target material according to preset deposition parameters. The preset deposition parameters include deposition gas pressure, deposition gas flow rate, deposition power, deposition time and deposition temperature. The deposition gas is generally nitrogen or a mixture of nitrogen and argon, that is, under vacuum conditions, the deposition gas pressure is 2 to 4×10 -2 Torr, deposition gas flow rate 200-500 sccm, deposition power 5-8 kW, deposition time 10-20 min, deposition temperature 380-550° C. Of course, those skilled in the art should understand that the range of the above preset values can be appropriately adjusted on the basis of achieving better deposition effect, depending on the actual situation.
[0063] It should be noted that in the process of physical vapor deposition of the metal layer on the inner surface of the pot body, in order to achieve the deposition of metal nitride particles, the deposition temperature is not less than 500°C to ensure that the metal and nitrogen can react normally to generate metal nitride particles. Therefore, it can be understood by those skilled in the art that in the process of physical vapor deposition to form a metal layer, the generation of metal particles and metal nitride particles can be controlled mainly by adjusting the deposition temperature to deposit and form a metal layer on the inner surface of the pot body.
[0064] Those skilled in the art can understand that in order to improve the non-stickiness and wear resistance of the metal layer, a physical vapor deposition process can be used to deposit metal particles on the inner surface of the pot body to form a metal film, and then the surface of the metal film away from the pot body is nitrided to reduce the surface energy of the metal film and improve the non-stick effect and wear resistance of the metal film. However, there are problems such as complex process operation and long production cycle. Preferably, a nitriding process is used, that is, a chemical heat treatment process that allows nitrogen atoms to penetrate into the surface of the metal film at a specific temperature and medium. Common processes include liquid nitriding, gas nitriding, ion nitriding, etc.
[0065] It should be noted that when metal particles are deposited only on the inner surface of the pot body by physical vapor deposition, argon gas may also be selected as the deposition gas.
[0066] It should be noted that when metal nitride particles are deposited on the inner surface of the pot body by physical vapor deposition, the target material can be selected from metal nitrides to directly form metal nitride particles for deposition during the physical vapor deposition process.
[0067] In an embodiment of the present invention, based on the fact that the metal layer will not chemically react with the food under high temperature heating and can maintain the original taste of the food, the target material can be selected from materials such as chromium, titanium, titanium-iron alloy, and titanium-aluminum alloy.
[0068] In the embodiment of the present invention, before the metal layer is prepared, the pot body is pre-treated in advance, including multi-stage vacuum and preheating treatment, and plasma cleaning. The multi-stage vacuum and preheating treatment is to place the pot body in a vacuum treatment chamber with 3-10 levels. After the pot body enters the vacuum treatment chamber, vacuum and preheating treatment are performed step by step. The pressure of the last stage chamber is 2-4×10 -2 Torr, and the temperature reaches 200-350°C to meet the requirements of subsequent physical vapor deposition coating.
[0069] Plasma cleaning is a process of removing impurities and organic matter by bombarding the surface of an object with ionized gas. It can deeply remove surface impurities, hydrocarbon dirt, etc., and create a high-density cross-linked layer, add polar functional groups, and improve the adhesion of the surface coating.
[0070] In the embodiment of the present invention, after the multi-stage vacuum and preheating treatments, the inner surface of the pot body is plasma cleaned.
[0071] According to the manufacturing method of the above-mentioned cookware, the inner pot of the rice cooker is manufactured: a stainless steel plate is used as the base material of the pot body, one side surface of the stainless steel plate is etched to form a rough surface with concave-convex patterns, the etched stainless steel plate is stretched to form a pot body, so that the concave-convex patterns are located on the inner surface of the pot body, and the inner surface of the pot body is subjected to physical vapor deposition to form a metal layer, and cookware 1#-11# and comparative cookware D1#-D4# are obtained. Among them, the metal layer is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, the metal nitride particles are at least partially filled in the gap micropores of the metal particles, the metal particles are chromium particles, and the metal nitride particles are chromium nitride particles; the concave-convex patterns include concave parts and convex ridges formed between two adjacent concave parts, and the concave parts are distributed in a lattice on the inner surface of the pot body. In Table 1, "-" represents no, and "√" represents yes.
[0072] Table 1
[0073]
[0074]
[0075] Using the manufacturing method of Example 2, pots 12#-14# are obtained, wherein the metal layer is a metal film formed by metal particles deposited on the inner surface of the pot body, and the metal film covers the surface of the film formed by the deposition of metal nitride particles. The specific differences are shown in Table 2.
[0076] Table 2
[0077]
[0078] Test example:
[0079] The non-stick properties, inner surface wear resistance and corrosion resistance of cookware 1#-14# and D1#-D5# were tested. The test results are shown in Table 3. The specific test methods are as follows:
[0080] Non-stickiness: Cook a medium amount of rice using the normal cooking procedure, turn the inner pot upside down and observe by gravity or by gently shaking. Wash (with a soft cloth) and repeat the test twice. If the non-stickiness level is above level 2 (including level 2) for all three times, it is considered qualified.
[0081] Non-stick rating criteria:
[0082] Level 0: No shaking required, all rice falls off
[0083] Level 1: Shake gently and all the rice falls off
[0084] Level 2: Gently shake, some rice still sticks to the surface (less than 1 / 3)
[0085] Level 3: Gently shaken, most areas are still covered with rice
[0086] Inner surface wear resistance: The sample is fixed on the wear tester, with a 3 kg weight and a scouring pad, and a 0.5% concentration of common detergent solution is added to soak the friction surface, and rubbed back and forth on the flat area, and the scouring pad is replaced every 500 times. 800 times without scratches or slight scratches (no more than 3 obvious scratches on the base material of the pot body) are judged as qualified, and more than 800 times with obvious scratches on the base material of the pot body are judged as unqualified.
[0087] Corrosion resistance: After spraying with 5% NaCl solution for 24 hours and then rinsing with tap water, if there is no obvious rust or corrosion, it is judged to be normal and qualified.
[0088] Table 3
[0089]
[0090]
[0091] According to the test data in Table 3, after the non-stickiness, inner surface wear resistance and corrosion resistance tests, the pots 1#-14# meet the non-stickiness, inner surface wear resistance and corrosion resistance requirements of the pots, among which the inner surfaces of pots 1#, 3# and 10# have slight scratches or no scratches, and the inner surfaces of pots 12#-14# have slight scratches. After the non-stickiness, inner surface wear resistance and corrosion resistance tests of pots D1#-D4#, the inner surfaces of pots D1# and D2# have obvious scratches and are unqualified, and the non-stickiness and inner surface wear resistance of pot D4# are unqualified.
[0092] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. An easy-to-clean cookware, characterized in that: include: A pot body, wherein the inner surface of the pot body is formed with concave-convex patterns; The metal layer is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles are at least partially filled in the gap micropores of the metal particles.
2. The easy-to-clean cookware according to claim 1, characterized in that: The metal particles are deposited to form a metal film, and the metal film covers the surface of the film formed by the deposition of the metal nitride particles.
3. The easy-to-clean cookware according to claim 1, characterized in that: The thickness of the metal layer is 0.5-1.5 μm.
4. The easy-to-clean cookware according to claim 1, characterized in that: The content of the metal nitride in the metal layer is 20-35 wt %.
5. The easy-to-clean cookware according to claim 1, characterized in that: The thickness of the metal layer in the area of the pot body flange is not less than the thickness of the metal layer in the area of the pot body bottom wall.
6. The easy-to-clean cookware according to claim 1, characterized in that: The concave-convex pattern includes concave parts and convex edges formed between two adjacent concave parts, and the concave parts are distributed on the inner surface of the pot body in a dot matrix.
7. A method for manufacturing an easy-to-clean cookware according to any one of claims 1 to 6, characterized in that: The steps include: S1: etching or mechanically punching the metal sheet so that a concave-convex pattern is formed on one side of the surface of the metal sheet; S2: stretching the metal sheet into a pot body so that the concave and convex patterns are located on the inner surface of the pot body; S3: Performing physical vapor deposition on the inner surface of the pot body to form a metal layer, wherein the metal layer is a thin film layer formed by the deposition of metal particles and metal nitride particles on the inner surface of the pot body, wherein the metal nitride particles at least partially fill the gap micropores of the metal particles.
8. The method for manufacturing an easy-to-clean cookware according to claim 7, characterized in that: The physical vapor deposition treatment method is: using a target material to deposit a metal layer on the inner surface of the pot body according to preset deposition parameters.
9. The method for manufacturing an easy-to-clean cookware according to claim 8, characterized in that: The preset deposition parameters include: deposition gas pressure, deposition gas flow rate, deposition power and deposition time, wherein the deposition gas pressure is 2 to 4×10 -2 Torr, deposition gas flow rate is 200-500 sccm, deposition power is 5-8 kW, and deposition time is 10-20 min.