Color developing element, preparation method of color developing element, magnetochromic ink and preparation method of magnetochromic ink

The superparamagnetic nanocolloid particles of long-chain polymers and hydrophobic small molecules are grafted through surface branches to form polymer brushes to ensure stable assembly of color development moieties, solving the unstable assembly of existing magnetochromic inks during packaging. Problem, wider discoloration range and higher color saturation and discoloration stability are achieved.

CN118904224APending Publication Date: 2024-11-08WUHAN XINGUANG TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958336.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing magnetochromic inks are susceptible to interference from external impurities, ions or solvent polarity during packaging, affecting their orderly assembly ability and magnetochromic effect, resulting in poor color discoloration range, color saturation and discoloration stability.

Method used

Superparamagnetic nanocolloid particles of surface branches grafted with long chain polymers and hydrophobic small molecules are formed to replace electrostatic repulsion, ensuring the dispersion and assembly stability of the color development moiety in different solvent systems, and through micro The capsule structure encapsulates the photonic crystal capsule core material, forming a color-producing element with steric repulsion force.

Benefits of technology

The long-term stable magnetochromic effect of the color development element is realized, the width of the color distortion range and the color saturation are enhanced, the stability of the color distortion cycle is improved, and the operation is simple, and it is suitable for printing and pattern formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904224A_ABST
    Figure CN118904224A_ABST
Patent Text Reader

Abstract

The invention discloses a color development element and a preparation method thereof, and magnetochromic ink and a preparation method thereof, the color development element comprises a microcapsule shell layer and a photonic crystal capsule core material located in the microcapsule shell layer, and the photonic crystal capsule core material comprises a dispersion liquid and superparamagnetic nano colloid particles dispersed in the dispersion liquid, long-chain polymers are grafted on the surfaces of the superparamagnetic nano colloid particles. Surface modification can be carried out on the superparamagnetic nano colloid particles by grafting hydrophobic small molecules on the long-chain polymer, so that the dispersibility of the particles in different solvent systems is ensured. The steric hindrance repulsive force generated by the polymer brush replaces the electrostatic repulsive force on the surface of the traditional magnetic element, so that the high saturation, wide response range and long-term stable magnetochromic effect of the structural color of the packaged developing element are ensured; under the same particle size, the super-paramagnetic nano colloid particle responds to a wider color changing range compared with the super-paramagnetic nano colloid particle not grafted with the long-chain polymer and the modified substance thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of intelligent color change, and more specifically, relates to a color developing element and a preparation method thereof, and a magnetochromic ink and a preparation method thereof. Background Art

[0002] Smart color-changing ink is a high-end color-changing material that can present different colors according to changes in external environmental conditions. It can significantly enhance the visual effect and added value of the product and has a wide range of applications in the fields of automotive coating, smart display, sensing and anti-counterfeiting. Color-changing ink based on responsive photonic crystals has a unique dynamic structural color effect, which originates from the selective diffraction of light by the internal coordinated nano-ordered structure, showing a series of advantages such as fast response, high saturation, environmental protection, and resistance to photobleaching.

[0003] Magnetically responsive photonic crystal materials are usually composed of superparamagnetic nanocolloidal particles dispersed in a solvent. Superparamagnetic nanocolloidal particles can be quickly assembled to form an ordered structure along the direction of an external magnetic field. By controlling the intensity and direction of the magnetic field, photonic crystal core materials can exhibit highly reversible structural color responses without damaging the ordered structure, making them an ideal choice for constructing magnetochromic inks. In existing studies, encapsulating magnetically responsive photonic crystal materials using microcapsule structures as magnetochromic primitives is an effective solution for constructing magnetochromic inks. However, conventional superparamagnetic nanocolloidal particles balance the magnetic attraction between particles through electrostatic repulsion, and are easily disturbed by external impurities, ions, or solvent polarity during the encapsulation process, thereby affecting the ordered assembly ability of the particles and the magnetochromic effect. How to avoid the reduction in the quality of structural color responsiveness (including magnetochromic range, structural color saturation, and color change stability) during the encapsulation of photonic crystal core materials is an urgent problem to be solved in the practical application of this type of color-changing ink. Summary of the invention

[0004] In view of the above defects or improvement needs of the prior art, the present invention provides a color-developing element and a preparation method, a magnetochromic ink and a preparation method, the purpose of which is to solve the defects of the existing color-developing element and magnetochromic ink in color change range, color saturation, color change stability and other aspects.

[0005] To achieve the above-mentioned purpose, according to one aspect of the present invention, a color-developing element is provided, comprising a microcapsule shell layer and a photonic crystal capsule core material located therein, wherein the photonic crystal capsule core material comprises a dispersion liquid and superparamagnetic nano-colloidal particles dispersed therein, and the surface of the superparamagnetic nano-colloidal particles is grafted with long-chain polymers. The surface of the superparamagnetic nano-colloidal particles can also be modified by grafting hydrophobic small molecules onto the long-chain polymer to ensure the dispersibility of the particles in different solvent systems.

[0006] Through the above technical solution, the steric repulsion generated by the formed polymer brush replaces the electrostatic repulsion on the surface of the traditional magnetic primitive. Its orderly assembly is not sensitive to external impurities, ions or solvent polarity, ensuring the saturation and color change cycle of the color-developing primitive structure color after encapsulation. These long-chain polymers combined with hydrophobic small molecules can help superparamagnetic nano-colloidal particles to be better dispersed in polyols and alkane solvents, so that the color-developing primitive has a long-term and stable magnetochromic effect. It can achieve a wider color change range than superparamagnetic nano-colloidal particles without grafted long-chain polymers and hydrophobic small molecules at the same particle size.

[0007] Preferably, the molecular weight of the long-chain polymer is 2k-100k, including one of polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone and polyvinyl pyridine, and the hydrophobic small molecule includes one of fatty acid with an alkyl chain carbon number greater than 8 and alkyl phenol.

[0008] Preferably, the average particle size of the superparamagnetic nano-colloidal particles is 50 to 300 nm, and the average particle size of the color-developing element is 5 to 300 μm.

[0009] According to another aspect of the present invention, there is also provided a method for preparing a color-developing element, comprising the following steps:

[0010] S1, taking superparamagnetic nanocolloid particles with long-chain polymers grafted on the surface, and grafting hydrophobic small molecules on the long-chain polymers;

[0011] S2, mixing the superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules with solvent A, and adding an initiator or a cross-linking agent to obtain a photonic crystal capsule core material;

[0012] S3, emulsifying the photonic crystal capsule core material with a solvent B containing a surfactant to obtain an emulsion;

[0013] S4, preparing a polymerization solution with a prepolymer and a solvent B, adding the polymerization solution to the emulsion, performing stirring polymerization, and forming a microcapsule shell layer on the surface of the photonic crystal capsule core material;

[0014] S5, separating, washing and drying the microcapsule shell layer in sequence to obtain the color-developing element.

[0015] Through the above technical scheme, it is possible to further graft hydrophobic small molecules onto superparamagnetic nano-colloidal particles with long-chain polymers grafted on the surface, and encapsulate them into a microcapsule structure to obtain a color-developing element.

[0016] Preferably, in S1, hydrophobic small molecules are grafted onto the long-chain polymer, specifically: superparamagnetic nano-colloidal particles with long-chain polymers grafted on the surface are mixed with hydrophobic small molecules and dispersed in a co-solvent, wherein the co-solvent includes one of dichloromethane, chloroform, tetrahydrofuran, ethyl acetate, and N,N-dimethylformamide, and stirred and separated in sequence to obtain superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules.

[0017] Preferably, in S2, the concentration of the superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules in the solvent A is 10-100 mg / mL, and the volume ratio of the photonic crystal core material to the solvent B is 1:5-1:150.

[0018] Preferably, the initiator is one of azobisisobutyronitrile, ammonium persulfate, and dibenzoyl peroxide;

[0019] The crosslinking agent is one or more of maleic anhydride, phthalic anhydride, terephthalic anhydride, ethylenediamine, 1,6-hexanediamine, urea, diethylenetriamine, diethylenetetramine, polyethyleneimine, aminoethylpiperazine, T-31 modified amine, m-phenylenediamine, dimethylthiotoluenediamine, and diaminodiphenylmethane;

[0020] The solvent A is one or more of ethylene glycol, glycerol, pentanediol, butylene glycol, 1,4-butanediol, 1,6-hexanediol, polyethylene glycol, pentaerythritol, inositol, sequoia alcohol, sinapyl alcohol, L-(-)-arabinitol, xylitol, and long-chain alkanes, wherein the long-chain alkanes are selected from n-octane to n-octadecane;

[0021] The solvent B is one or more of benzene, toluene, xylene, carbon tetrachloride, ethylene dichloride, chlorobenzene, liquid paraffin, and water;

[0022] The surfactant is one or more of alkylphenol polyoxyethylene ether, ethylene glycol fatty acid ester, propylene glycol fatty acid ester, glyceryl monostearate, sorbitan monostearate, polyoxyethylene oleyl alcohol ether diethylene glycol fatty acid ester, diethylene glycol monolaurate, fatty alcohol polyoxyethylene ether, hydroxylated lanolin, polyoxyethylene sorbitol beeswax derivative, cetyl polyethylene glycol, polyoxyethylene dioleate, tetraethylene glycol monostearate, polyvinyl alcohol, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, Span series, and Tween series.

[0023] Preferably, the prepolymer is any one of styrene, methyl methacrylate, isoprene, diethyl carbonate, toluene-2,6-diisocyanate, hexamethylene diisocyanate, toluene-2,4-diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, bisphenol A type epoxy resin prepolymer, and propylene oxide type epoxy resin prepolymer.

[0024] According to another aspect of the present invention, a magnetochromic ink is provided, comprising the aforementioned color-developing element and a functional resin, wherein the color-developing element is dispersed in the functional resin.

[0025] By means of the above technical solution, the color-developing element of the present invention can be made into magnetochromic ink.

[0026] According to another aspect of the present invention, a method for preparing a magnetochromic ink is provided, comprising the method for preparing the aforementioned color-developing element, and further comprising S5, dispersing the color-developing element in a functional resin to obtain the magnetochromic ink, wherein the functional resin is any one or more of an acrylic resin, an epoxy resin, a polyurethane resin, a polycarbonate resin, and a silicone resin.

[0027] In general, the beneficial effects of the present invention are as follows:

[0028] (1) As a new type of color-changing ink, the pattern formed by its printing can show bright structural colors under the action of a conventional external magnetic field, and the color can be continuously adjusted with the change of the magnetic field. Compared with existing magnetochromic inks, it has the advantages of a wide color change range, high color saturation, and excellent color change cycle stability.

[0029] (2) The powdered product obtained after centrifugation, washing and drying, namely the color-developing element, is easy to store stably. The powdered substance is redispersed in a curable medium to obtain a stable and uniform magnetochromic ink.

[0030] (3) The microcapsule structure of the present invention has high sealing performance and is not prone to adhesion. The capsule size is easy to control and the light-transmitting wall layer material can be flexibly selected according to different ink medium systems.

[0031] (4) The preparation method of the color-developing element and the magnetochromic ink in the present invention is simple to operate and has mild reaction conditions. The entire process of some embodiments can be completed at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 These are digital photos of the photonic crystal core material in Example 1 under different magnetic field strengths (a) 450 Gs, (b) 250 Gs, and (c) 100 Gs;

[0033] Figure 2 These are optical microscope photos of the color-developing element dispersed in the polyurethane resin in Example 1 when (a) no magnetic field is applied and (b) a magnetic field is applied;

[0034] Figure 3 : is the diffraction spectrum of the magnetochromic ink in Example 1 under different magnetic field intensities;

[0035] Figure 4 are digital photographs of the magnetochromic ink in Example 1 after coating to form a solid sheet in (a) no magnetic field is applied and (b) a magnetic field is applied;

[0036] Figure 5 : is the diffraction spectrum of the magnetochromic ink in Example 2 under different magnetic field intensities;

[0037] Figure 6 : is the diffraction spectrum of the magnetochromic ink in Example 3 under different magnetic field intensities;

[0038] Figure 7 : is the diffraction spectrum of the magnetochromic ink in Example 4 under different magnetic field intensities;

[0039] Figure 8 is the diffraction spectrum of the magnetochromic ink in Example 5 under different magnetic field intensities;

[0040] Fig. 9 : Diffraction spectra of the magnetochromic ink in Example 6 under different magnetic field intensities. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0042] The present invention provides a color-developing element, comprising a microcapsule shell layer and a photonic crystal capsule core material located therein, wherein the photonic crystal capsule core material comprises a dispersion liquid and superparamagnetic nano-colloidal particles dispersed therein, the surface of the superparamagnetic nano-colloidal particles is grafted with a long-chain polymer, and the long-chain polymer can also be grafted with a hydrophobic small molecule.

[0043] In the Chinese patent with publication number CN103342393A, it is disclosed that long-chain polymer polyvinyl pyrrolidone is grafted on superparamagnetic nano-colloidal particles. The present invention further grafts hydrophobic small molecules on the basis of long-chain polymers, and performs surface modification on superparamagnetic nano-colloidal particles to ensure the dispersibility of particles in different solvent systems. The steric repulsion generated by the formed polymer brush replaces the electrostatic repulsion on the surface of the traditional magnetic primitive, and its orderly assembly is not sensitive to external impurities, ions or solvent polarity, which ensures the saturation, wide response range and color change cycle stability of the color-developing primitive structure color after encapsulation. A certain magnetic field is applied to the encapsulated color-developing primitive, and the superparamagnetic nano-colloidal particles dispersed in the photonic crystal capsule core material can be one-dimensionally oriented and orderly assembled along the direction of the applied magnetic field, and changing the magnetic field intensity can change the spacing between adjacent superparamagnetic nano-colloidal particles, thereby affecting the wavelength of reflected light and achieving the effect of magnetochromism.

[0044] In some embodiments, the molecular weight of the long-chain polymer is 2k to 100k, including one of polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone, and polyvinyl pyridine. These long-chain polymers can help superparamagnetic nano-colloidal particles to be better dispersed in polyol solvents. The hydrophobic small molecule is one of fatty acids and alkylphenols with an alkyl chain carbon number greater than 8. Among them, the fatty acid with an alkyl chain carbon number greater than 8 can be selected from: oleic acid, myristic acid, and capric acid, and the alkylphenol can be selected from: pentadecylphenol and dodecylphenol. For example, oleic acid can be grafted on polyvinyl pyrrolidone, and pentadecylphenol can be grafted on polyvinyl pyridine. In addition to polyvinyl pyrrolidone in the prior art, the long-chain polymer of the present invention can also use polyvinyl alcohol, polyethylene glycol, and polyvinyl pyridine. These long-chain polymers combined with hydrophobic small molecules can help superparamagnetic nano-colloidal particles to be better dispersed in alkane solvents, so that the color-developing element has a long-term and stable magnetochromic effect. Different types of long-chain polymers have different extension degrees in the same solvent, thereby achieving the effect of changing the corresponding range of the color-developing element magnetism. Based on the selection of the long-chain polymer and the hydrophobic small molecule, the solvent A in the present invention can be selected from polyols and alkane solvents alone or in combination.

[0045] Furthermore, the average particle size of the superparamagnetic nano-colloidal particles is 50 to 300 nm, and the average particle size of the color-developing primitive is 5 to 300 μm. The superparamagnetic nano-colloidal particles of the present invention contain at least one element of iron, cobalt, and nickel. The particle size control of the superparamagnetic nano-colloidal particles determines the main color change range of the material. The smaller particle size changes with blue as the center, the larger particle size changes with green as the center, and the larger particle size changes with red as the center. The particle size of the color-developing primitive determines the limitations of its subsequent use. The larger particle size can only be printed by coating and the like, and the visual resolution is low. The small-sized particle size can be suitable for efficient methods such as screen printing and printing, and the printed pattern has good continuity. The average particle size of the superparamagnetic nano-colloidal particles of the present invention can cover the color change range of visible light, and the average particle size of the color-developing primitive of the present invention is suitable for efficient application scenarios such as screen printing, and has better continuity. On the premise that the average particle size has the above-mentioned advantages, the present invention can achieve a wider color change range than superparamagnetic nano-colloidal particles without the grafting of the aforementioned long-chain polymers and hydrophobic small molecules at the same particle size due to the grafting of the aforementioned long-chain polymers and hydrophobic small molecules on the surface of the superparamagnetic nano-colloidal particles and the selection of polyols and alkane solvents.

[0046] The present invention also provides a method for preparing a color-developing element, comprising the following steps:

[0047] S1, taking superparamagnetic nanocolloid particles with long-chain polymers grafted on the surface, and grafting hydrophobic small molecules on the long-chain polymers;

[0048] S2, mixing the superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules with solvent A, and adding an initiator or a cross-linking agent to obtain a photonic crystal capsule core material;

[0049] S3, emulsifying the photonic crystal capsule core material with a solvent B containing a surfactant to obtain an emulsion;

[0050] S4, preparing a polymerization solution with a prepolymer and a solvent B, adding the polymerization solution to the emulsion, performing stirring polymerization, and forming a microcapsule shell layer on the surface of the photonic crystal capsule core material;

[0051] S5, separating, washing and drying the microcapsule shell layer in sequence to obtain the color-developing element.

[0052] In some embodiments, the long-chain polymer includes one of polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone, and polyvinyl pyridine. Specifically, the Chinese patent with publication number CN103342393A records how to graft the long-chain polymer polyvinyl pyrrolidone on the surface of superparamagnetic nanocolloidal particles. The grafting method of polyvinyl alcohol, polyethylene glycol, and polyvinyl pyrrolidone is similar to that of polyvinyl pyrrolidone, which will not be repeated here.

[0053] Furthermore, the hydrophobic small molecule includes one of a fatty acid and an alkylphenol with an alkyl chain carbon number greater than 8. Among them, the fatty acid with an alkyl chain carbon number greater than 8 can be selected from: oleic acid, myristic acid, and capric acid, and the alkylphenol can be selected from: pentadecylphenol and dodecylphenol. In S1, the step of grafting hydrophobic small molecules on the long-chain polymer is specifically: superparamagnetic nanocolloidal particles with long-chain polymers grafted on the surface are mixed with hydrophobic small molecules and dispersed in a co-solvent, and the co-solvent can be selected from: dichloromethane, chloroform, tetrahydrofuran, ethyl acetate, N, N-dimethylformamide, and stirred and separated in turn to obtain superparamagnetic nanocolloidal particles grafted with hydrophobic small molecules. In some embodiments, the stirring temperature can be selected at 30°C and stirred for 12 hours.

[0054] Furthermore, in S2, the concentration of the superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules in the solvent A is 10-100 mg / mL, and the volume ratio of the photonic crystal core material to the solvent B is 1:5-1:150.

[0055] Further, the solvent A is one or more of ethylene glycol, glycerol, pentanediol, butylene glycol, 1,4-butanediol, 1,6-hexanediol, polyethylene glycol, pentaerythritol, inositol, sequoia alcohol, sinapyl alcohol, L-(-)-arabinitol, xylitol, and long-chain alkanes, wherein the long-chain alkanes are selected from n-octane to n-octadecane.

[0056] Solvent A is used as a dispersion liquid in the color-developing element to disperse superparamagnetic nano-colloidal particles to construct a stable emulsion system. The color-developing element of the present invention is a microcapsule structure. In order to meet the requirements of rapid and stable magnetochromism, the photonic crystal capsule core material in the microcapsule structure is determined to be a colorless solvent with low volatility and low viscosity as a dispersion liquid, and can be used as a dispersed phase to form a stable emulsion. The present invention selects polyols as a dispersed phase to form an oil-in-alcohol emulsion, and selects long-chain alkanes as a dispersed phase to form an oil-in-water emulsion. In combination with superparamagnetic nano-colloidal particles grafted with long-chain polymers and hydrophobic small molecules, the particles can be better dispersed in the above-mentioned dispersion liquid.

[0057] Furthermore, an initiator or a crosslinking agent is added in S2, and the solvent A can be used as a dispersion liquid. The photonic crystal capsule core material formed in this way can form a stable emulsion system dispersed phase after being treated in S3. In addition, the crosslinking agent and the initiator are also used to form a microcapsule shell layer in the subsequent S4.

[0058] Specifically, the initiator is one of azobisisobutyronitrile, ammonium persulfate, and dibenzoyl peroxide. The crosslinking agent is one or more of maleic anhydride, phthalic anhydride, terephthalic anhydride, ethylenediamine, 1,6-hexanediamine, urea, diethylenetriamine, diethylenetetramine, polyethyleneimine, aminoethylpiperazine, T-31 modified amine, m-phenylenediamine, dimethylthiotoluenediamine, and diaminodiphenylmethane.

[0059] Further, in S3, the photonic crystal capsule core material is emulsified using a solvent B containing a surfactant, and the solvent B is one or more of benzene, toluene, xylene, carbon tetrachloride, ethylene dichloride, chlorobenzene, liquid paraffin, and water. In some embodiments, when the solvent A is a polyol solvent, the solvent B selects one or more of benzene, toluene, xylene, carbon tetrachloride, ethylene dichloride, chlorobenzene, and liquid paraffin as a continuous phase for emulsification to obtain an emulsion; in other embodiments, when the solvent A is a long-chain alkane solvent, water can be used as a continuous phase in the solvent B for emulsification to obtain an emulsion.

[0060] Described surfactant is one or more in alkylphenol polyoxyethylene ether, ethylene glycol fatty acid ester, propylene glycol fatty acid ester, glyceryl monostearate, sorbitan monostearate, polyoxyethylene oleyl alcohol ether diethylene glycol fatty acid ester, diethylene glycol monolaurate, fatty alcohol polyoxyethylene ether, hydroxylated lanolin, polyoxyethylene sorbitol beeswax derivative, cetyl polyethylene glycol, polyoxyethylene dioleate, tetraethylene glycol monostearate, Span series, these belong to water-in-oil or alcohol-in-oil surfactant. In addition, surfactant can also be water-in-oil, for example one or more in polyvinyl alcohol, sodium lauryl sulfate, hexadecyl trimethyl ammonium bromide, Tween series. According to solvent A, solvent B, select corresponding surfactant, and the alcohol-in-oil emulsion or water-in-oil emulsion formed will be more stable.

[0061] Furthermore, S4 is based on the emulsion system of S3, and polymerization is carried out to construct a microcapsule shell layer. The polymerization solution is slowly added to the emulsion, and the polymerization can be carried out by continuous stirring for 0.2h-4h. The polymerization needs to select an appropriate polymer material, specifically, the prepolymer is any one of styrene, methyl methacrylate, isoprene, diethyl carbonate, toluene-2,6-diisocyanate, hexamethylene diisocyanate, toluene-2,4-diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, bisphenol A type epoxy resin prepolymer, and propylene oxide type epoxy resin prepolymer.

[0062] More specifically, when styrene is selected as the prepolymer, the microcapsule shell material formed is polystyrene; when methyl methacrylate is selected as the prepolymer, the microcapsule shell material formed is polymethyl methacrylate; when isoprene is selected as the prepolymer, the microcapsule shell material formed is polyisoprene; when diethyl carbonate is selected as the prepolymer, the microcapsule shell material formed is polycarbonate; when toluene-2,6-diisocyanate, hexamethylene diisocyanate, toluene-2,4-diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate are selected as prepolymers, the microcapsule shell material formed is polyurea or polyurethane; when bisphenol A type epoxy resin prepolymer or propylene oxide type epoxy resin prepolymer is selected as the prepolymer, the microcapsule shell material formed is epoxy resin. Therefore, when one or more of the materials listed above are selected as prepolymers, the shell material of the formed microcapsule is any one or more of polymethyl methacrylate, polystyrene, polycarbonate, polyisoprene, polyurea, polyurethane, and epoxy resin.

[0063] The prepolymer, initiator or cross-linking agent required for polymerization can be dissolved in at least one of the inner and outer phases of the emulsion. The reactants can be in the inner and outer phases respectively, for example, the isocyanate and diamine required for preparing the polyurea shell layer are dissolved in the outer phase and the inner phase respectively; or they can be both in the outer phase, for example, the diethyl carbonate and terephthalic anhydride required for preparing the polycarbonate shell layer are both dissolved in the outer phase xylene solution; finally, the microcapsule shell layer is polymerized at the interface of the emulsion droplets through interfacial polymerization or in-situ polymerization, which is insoluble in any of the inner and outer phases of the emulsion and has light transmittance, stability, sealing, and good mechanical strength.

[0064] Furthermore, the microcapsule shell is sequentially separated, washed, and dried. The microcapsule shell encapsulates an initiator or a crosslinking agent, and also encapsulates a solvent A and superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules. The initiator or the crosslinking agent and the solvent A are used as a dispersion liquid to disperse the superparamagnetic nano-colloidal particles. The microcapsule shell and the internal encapsulation form a whole microcapsule structure of the color-developing element, and finally the color-developing element is obtained. The dispersed superparamagnetic nano-colloidal particles are assembled in one dimension along the direction of the external magnetic field, and the magnetic attraction is balanced by the steric repulsion of the polymer on the particle surface to form an ordered structure, thereby achieving the purpose of color development.

[0065] The present invention also provides a magnetochromic ink, comprising the aforementioned color-developing element and a functional resin, wherein the color-developing element is dispersed in the functional resin.

[0066] The present invention also proposes a method for preparing a magnetochromic ink, including the method for preparing the aforementioned color-developing element, and also includes S6, dispersing the color-developing element in a functional resin to obtain the magnetochromic ink, wherein the functional resin is any one or more of an acrylic resin, an epoxy resin, a polyurethane resin, a polycarbonate resin, and a silica gel resin.

[0067] The color-developing element obtained by S5 is in the form of a powder with a microcapsule structure. It is dispersed in a functional resin to obtain a magnetochromic ink, which can be used to prepare printed products with anti-counterfeiting functions. The functional resin has properties such as light transmission, hydrophobicity, wear resistance, etc., and can be a flexible or rigid material. The functional resin selected by the present invention will not significantly affect the magnetic response speed, color change range and structural color saturation of the color-developing element before and after coating.

[0068] In a specific embodiment, the emulsion system is of oil-in-alcohol type, using alcohol-soluble superparamagnetic nano-colloidal particles. The photonic crystal capsule core material is selected from superparamagnetic nano-colloidal particles with polyethylene glycol grafted on the surface, a polyamine cross-linking agent selected from the aforementioned cross-linking agent materials, and a polyol dispersion liquid, and the microcapsule shell layer is selected from polyurea formed by polycondensation reaction of isocyanate substances and polyamines, and polyurethane formed by polycondensation reaction of isocyanate substances and polyols; further selected, the isocyanate substance is hexamethylene diisocyanate, the polyamine substance is 1,6-hexanediamine, the polyol substance is sequoia alcohol, and the functional resin is a polyurethane resin. Under the stimulation of a magnetic field with an intensity of 100 to 500 Gs, the magnetochromic ink exhibits a diffraction peak in the range of 623 nm to 435 nm and a reversible change of the corresponding structural color. The magnetochromic ink has the characteristics of rapid magnetic response (about 100 ms), a wide color change range, high color saturation, and excellent color change cycle (stable structural color change phenomenon occurred in 5000 cycles of applying / removing the magnetic field).

[0069] In another specific embodiment, the emulsion system is of the oil-in-water type, so fat-soluble superparamagnetic nano-colloidal particles are used. The photonic crystal capsule core material is selected to be composed of superparamagnetic nano-colloidal particles of polyvinyl pyrrolidone modified by oleic acid grafted on the surface and hexadecane dispersion, the prepolymer of the microcapsule shell layer is methyl methacrylate, the initiator substance is ammonium persulfate, and the functional resin is an acrylic resin. In this embodiment, the microcapsule shell layer is formed by a free radical polymerization reaction of a monomer having a carbon-carbon double bond initiated by an initiator at the interface of the emulsion droplet. Under the stimulation of a magnetic field with an intensity of 100 to 450 Gs, the magnetochromic ink exhibits a diffraction peak in the range of 710 to 491 nm and a reversible change of the corresponding structural color. The magnetochromic ink has the characteristics of rapid magnetic response (about 100 ms), wide color change range, high color saturation, and excellent color change cycle (in 5000 cycles of applying / removing the magnetic field, stable structural color changes occurred).

[0070] The following examples all use superparamagnetic nano-colloidal particles of Fe(1-yz)CozNiyOx.

[0071] Example 1

[0072] (1) Superparamagnetic nano-colloidal particles (average particle size of 150 nm) with polyvinyl pyrrolidone grafted on the surface were dispersed in red taxol, and a certain amount of 1,6-hexanediamine was added to obtain a photonic crystal core material with a concentration of 100 mg / ml. Its responsiveness is as follows Figure 1 As shown, it can be seen that different structural colors are exhibited under different magnetic field strengths. In the figure, (a) is 450Gs, (b) is 250Gs, and (c) is 100Gs. Then it is added to a xylene solution containing a surfactant (cetyl polyethylene glycol) and stirred to form a uniform emulsion. The volume ratio of the photonic crystal core material to the xylene solution is 1:50.

[0073] (2) The obtained emulsion is placed in a reaction container, and a chlorobenzene solution containing hexamethylene diisocyanate is slowly added thereto, and the polymerization is carried out by continuous stirring at room temperature for 1 hour.

[0074] (3) The solution obtained after polymerization is centrifuged, washed and dried to obtain polyurea-polyurethane microcapsules, i.e., color-forming elements, with an average particle size of 50 μm. The obtained color-forming elements are collected and dispersed in polyurethane resin to form magnetochromic ink, such as Figure 2 As shown in the figure, (a) is without magnetic field, (b) is with magnetic field, it can be seen that the microcapsule structure is still completely maintained. At the same time, the prepared magnetochromic ink shows a reversible change of diffraction peaks in the range of 623 to 435 nm and corresponding structural colors under the stimulation of a magnetic field with an intensity of 100 to 500 Gs. Its responsiveness is shown in Figure 3As shown in the figure, it can be seen that the photonic crystal core material still maintains a wide magnetochromic range and high reflectivity after encapsulation. The polyurethane sheet formed by the magnetochromic ink after coating and curing can show obvious magnetochromic effect, such as Figure 4 As shown in the figure, (a) is without magnetic field, and (b) is with magnetic field. In the experiment of applying / removing magnetic field 5000 times, the thin film showed stable structural color change phenomenon.

[0075] Example 2

[0076] (1) Superparamagnetic nano-colloidal particles (average particle size of 180 nm) of polyvinyl pyrrolidone modified by grafting oleic acid on the surface are dispersed in hexadecane to obtain a photonic crystal capsule core material with a concentration of 50 mg / ml. Then, the superparamagnetic nano-colloidal particles are added to an aqueous solution containing a surfactant (polyvinyl alcohol) and ammonium persulfate and stirred to form a uniform emulsion. The volume ratio of the photonic crystal capsule core material to the aqueous solution is 1:100.

[0077] (2) The obtained emulsion was placed in a reaction container, and an aqueous solution containing methyl methacrylate was slowly added thereto, and the mixture was continuously stirred at 70° C. for 2 h to carry out polymerization.

[0078] (3) The solution obtained after polymerization is centrifuged, washed and dried to obtain polymethyl methacrylate microcapsules, i.e., color-developing elements. The average particle size is 40 μm. Under the stimulation of a magnetic field with an intensity of 100 to 450 Gs, the magnetochromic ink made of the color-developing element exhibits a diffraction peak in the range of 710 to 491 nm and a reversible change in the corresponding structural color. Its responsiveness is as follows: Figure 5 shown.

[0079] Example 3

[0080] (1) Superparamagnetic nano-colloidal particles (average particle size of 160 nm) with surface grafted polyvinyl alcohol are dispersed in ethylene glycol, and a certain amount of ethylenediamine is added to obtain a photonic crystal core material with a concentration of 50 mg / ml. Then, the material is added to a chlorobenzene solution containing a surfactant (Span 60) and stirred to form a uniform emulsion. The volume ratio of the photonic crystal core material to the chlorobenzene solution is 1:25.

[0081] (2) The obtained emulsion was placed in a reaction container, and a chlorobenzene solution containing bisphenol A epoxy resin S-28 was slowly added, and the mixture was continuously stirred at 50° C. for 3 h to carry out polymerization.

[0082] (3) The obtained solution after polymerization is centrifuged, washed and dried to obtain epoxy resin microcapsules, i.e., color-developing elements. The average particle size is 100 μm. Under the stimulation of a magnetic field with an intensity of 100 to 420 Gs, the magnetochromic ink made of the color-developing element exhibits a diffraction peak in the range of 640 to 428 nm and a reversible change in the corresponding structural color. Its responsiveness is as follows: Figure 6 shown.

[0083] Example 4

[0084] (1) Superparamagnetic nanocolloid particles (average particle size of 200 nm) with polyethylene glycol grafted on the surface are dispersed in polyethylene glycol 400, and a certain amount of polyethyleneimine is added to obtain a photonic crystal core material with a concentration of 40 mg / ml. Then, the material is added to a dichloroethane solution containing a surfactant (Span 80) and stirred to form a uniform emulsion. The volume ratio of the photonic crystal core material to the dichloroethane solution is 1:25.

[0085] (2) The obtained emulsion is placed in a reaction container, and a dichloroethane solution containing toluene-2,6-diisocyanate is slowly added thereto, and the polymerization is carried out by continuous stirring at room temperature for 3 hours.

[0086] (3) The solution obtained after polymerization is centrifuged, washed and dried to obtain polyurea-polyurethane microcapsules, i.e., color-developing elements. The average particle size is 90 μm. Under the stimulation of a magnetic field with an intensity of 100 to 420 Gs, the magnetochromic ink made of the color-developing element exhibits a diffraction peak in the range of 756 to 535 nm and a reversible change in the corresponding structural color. Its responsiveness is as follows: Figure 7 shown.

[0087] Example 5

[0088] (1) Superparamagnetic nano-colloidal particles (average particle size of 130 nm) of polyvinyl pyridine modified with pentadecylphenol grafted on the surface and isoprene are dispersed in tetradecane to obtain a photonic crystal core material with a concentration of 50 mg / ml. Then, the material is added to an aqueous solution containing a surfactant (sodium dodecyl sulfate) and stirred to form a uniform emulsion. The volume ratio of the photonic crystal core material to the aqueous solution is 1:100.

[0089] (2) The obtained emulsion was placed in a reaction container, and a chlorobenzene solution of azobisisobutyronitrile was slowly added, and the polymerization was carried out by continuous stirring at room temperature for 3 hours.

[0090] (3) The solution obtained after polymerization is centrifuged, washed and dried to obtain polyisoprene microcapsules, i.e., color-developing elements. The average particle size is 40 μm. Under the stimulation of a magnetic field with an intensity of 100 to 380 Gs, the magnetochromic ink made of the color-developing element exhibits a diffraction peak in the range of 608 to 421 nm and a reversible change in the corresponding structural color. Its responsiveness is as follows: Figure 8 shown.

[0091] Example 6

[0092] (1) Superparamagnetic nano-colloidal particles (average particle size of 170 nm) with polyvinyl alcohol grafted on the surface are dispersed in glycerol to obtain a photonic crystal capsule core material with a concentration of 50 mg / ml. Then, the photonic crystal capsule core material is added to xylene containing a surfactant (propylene glycol fatty acid ester) and stirred to form a uniform emulsion. The volume ratio of the photonic crystal capsule core material to the xylene solution is 1:50.

[0093] (2) The obtained emulsion was placed in a reaction container, and a xylene solution of diethyl carbonate and terephthalic anhydride was slowly added, and the mixture was continuously stirred at 60° C. for 3 h to carry out polymerization.

[0094] (3) The solution obtained after polymerization is centrifuged, washed and dried to obtain polycarbonate microcapsules, i.e., the color-developing element of the magnetochromic ink. The average particle size is 50 μm. Under the stimulation of a magnetic field with an intensity of 100 to 450 Gs, the magnetochromic ink exhibits a diffraction peak in the range of 721 to 490 nm and a reversible change in the corresponding structural color. Its responsiveness is as follows: Fig. 9 shown.

[0095] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A color-developing element, characterized in that: It comprises a microcapsule shell layer and a photonic crystal capsule core material therein, wherein the photonic crystal capsule core material comprises a dispersion liquid and superparamagnetic nano-colloidal particles dispersed therein, the surface of the superparamagnetic nano-colloidal particles is grafted with a long-chain polymer, and the long-chain polymer is also grafted with a hydrophobic small molecule.

2. The color-developing element according to claim 1, characterized in that: The molecular weight of the long-chain polymer is 2k-100k, and includes one of polyvinyl alcohol, polyethylene glycol, polyvinyl pyrrolidone, and polyvinyl pyridine. The hydrophobic small molecule includes one of fatty acid with an alkyl chain carbon number greater than 8 and alkyl phenol.

3. The color-developing element according to claim 1, characterized in that: The average particle size of the superparamagnetic nano-colloidal particles is 50-300 nm, and the average particle size of the color-developing element is 5-300 μm.

4. A method for preparing a color-developing element, characterized in that: The following steps are involved: S1, taking superparamagnetic nanocolloid particles with long-chain polymers grafted on the surface, and grafting hydrophobic small molecules on the long-chain polymers; S2, mixing the superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules with solvent A, and adding an initiator or a cross-linking agent to obtain a photonic crystal capsule core material; S3, emulsifying the photonic crystal capsule core material with a solvent B containing a surfactant to obtain an emulsion; S4, preparing a polymerization solution with a prepolymer and a solvent B, adding the polymerization solution to the emulsion, performing stirring polymerization, and forming a microcapsule shell layer on the surface of the photonic crystal capsule core material; S5, separating, washing and drying the microcapsule shell layer in sequence to obtain the color-developing element.

5. The preparation method according to claim 4, characterized in that: In S1, hydrophobic small molecules are grafted onto the long-chain polymer, specifically: superparamagnetic nano-colloidal particles with long-chain polymers grafted on the surface are mixed with hydrophobic small molecules and dispersed in a co-solvent, wherein the co-solvent includes one of dichloromethane, chloroform, tetrahydrofuran, ethyl acetate, and N,N-dimethylformamide, and stirred and separated in sequence to obtain superparamagnetic nano-colloidal particles grafted with hydrophobic small molecules.

6. The preparation method according to claim 4, characterized in that: In S2, the concentration of the superparamagnetic nano-colloidal particles in the solvent A is 10-100 mg / mL, and the volume ratio of the photonic crystal core material to the solvent B is 1:5-1:

150.

7. The preparation method according to claim 5, characterized in that: The initiator is one of azobisisobutyronitrile, ammonium persulfate, and dibenzoyl peroxide; The crosslinking agent is one or more of maleic anhydride, phthalic anhydride, terephthalic anhydride, ethylenediamine, 1,6-hexanediamine, urea, diethylenetriamine, diethylenetetramine, polyethyleneimine, aminoethylpiperazine, T-31 modified amine, m-phenylenediamine, dimethylthiotoluenediamine, and diaminodiphenylmethane; The solvent A is one or more of ethylene glycol, glycerol, pentanediol, butylene glycol, 1,4-butanediol, 1,6-hexanediol, polyethylene glycol, pentaerythritol, inositol, sequoia alcohol, sinapyl alcohol, L-(-)-arabinitol, xylitol, and long-chain alkanes, wherein the long-chain alkanes are selected from n-octane to n-octadecane; The solvent B is one or more of benzene, toluene, xylene, carbon tetrachloride, ethylene dichloride, chlorobenzene, liquid paraffin, and water; The surfactant is one or more of alkylphenol polyoxyethylene ether, ethylene glycol fatty acid ester, propylene glycol fatty acid ester, glyceryl monostearate, sorbitan monostearate, polyoxyethylene oleyl alcohol ether diethylene glycol fatty acid ester, diethylene glycol monolaurate, fatty alcohol polyoxyethylene ether, hydroxylated lanolin, polyoxyethylene sorbitol beeswax derivative, cetyl polyethylene glycol, polyoxyethylene dioleate, tetraethylene glycol monostearate, polyvinyl alcohol, sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, Span series, and Tween series.

8. The preparation method according to claim 6, characterized in that: The prepolymer is any one of styrene, methyl methacrylate, isoprene, diethyl carbonate, toluene-2,6-diisocyanate, hexamethylene diisocyanate, toluene-2,4-diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, bisphenol A type epoxy resin prepolymer, and propylene oxide type epoxy resin prepolymer.

9. A magnetochromic ink, characterized in that: It comprises the color-developing element as described in any one of claims 1 to 3, and also comprises a functional resin, wherein the color-developing element is dispersed in the functional resin.

10. A method for preparing a magnetochromic ink, characterized in that: The method comprises the preparation method as described in any one of claims 4 to 8, and further comprises S6, dispersing the color-developing element in a functional resin to obtain the magnetochromic ink, wherein the functional resin is any one or more of an acrylic resin, an epoxy resin, a polyurethane resin, a polycarbonate resin, and a silicone resin.