Continuous homogeneous production equipment and production method of acrylonitrile polymer for PAN carbon fiber precursor

Through continuous homogeneous production equipment and methods, the spaced polymerization reaction and double-stage vacuum process are used to solve the problems of long production cycle and high energy consumption in the traditional PAN carbon fiber production process, improve the quality and production efficiency of polymers, and achieve more Efficient production of PAN carbon fiber raw silk.

CN118904258APending Publication Date: 2024-11-08ZHEJIANG JINGGONG SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411195591.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The traditional PAN carbon fiber production process has problems such as long production cycle, high energy consumption, large solid investment, low production capacity and batch differences, which affect the quality of the raw silk and subsequent process efficiency.

Method used

Continuous homogeneous production equipment and methods including preparation tanks, first and second polymerization kettles, despairing towers, despairing towers and spinning liquid delivery pumps are adopted, and the spaced polymerization reaction, double-stage vacuum process and low-temperature refrigeration water control is used. , high molecular weight PAN carbon fiber raw silk is produced.

Benefits of technology

Achieve shorter polymerization reaction time, reduce downtime and energy consumption, improve production efficiency and polymer quality, reduce the energy consumption of equipment preheating, and ensure single-single and foaming through the secondary vacuum process. Effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904258A_ABST
    Figure CN118904258A_ABST
Patent Text Reader

Abstract

The invention discloses continuous homogeneous production equipment and a production method of an acrylonitrile polymer for a PAN carbon fiber precursor, and belongs to the technical field of carbon fiber production equipment. Production equipment comprises a preparation tank, an output pipeline of the preparation tank is respectively connected with a first polymerization kettle and a second polymerization kettle, and the production method comprises the following steps: putting 21.88% of a first monomer acrylonitrile, 0.22% of a second monomer itaconic acid, 0.27% of a third monomer methyl acrylate and 77.37% of a solvent dimethyl sulfoxide into the preparation tank according to the weight ratio, and stirring; according to the invention, the first polymerization kettle and the second polymerization kettle are arranged to carry out continuous polymerization reaction, so that a polymer needing super-long polymerization reaction can be rapidly produced through the second polymerization kettle after being produced by controlling the first polymerization kettle, and the time of the first polymerization kettle and the time of the second polymerization kettle are separated, so that the production efficiency is improved within a shorter time. And more polymers are generated, so that the whole subsequent process can be continuously operated, and the shutdown waiting time is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber production equipment, and specifically relates to a continuous homogeneous production equipment and a production method for acrylonitrile polymer for PAN carbon fiber precursor. Background Art

[0002] Carbon fiber is a fibrous graphite material with a carbon content of more than 90%. It has the advantages of high axial strength and modulus, low density, good fatigue resistance, good corrosion resistance, etc. To prepare high-performance carbon fiber, the quality of the raw yarn is the key. The quality of the spinning solution directly determines the quality of the raw yarn. Therefore, obtaining a PAN solution with excellent performance becomes the source of influence on subsequent processes.

[0003] The traditional production process uses intermittent polymerization, which has problems such as long production cycle, high energy consumption, large solid investment, low production capacity, and differences between batches. Summary of the invention

[0004] The present invention mainly solves the technical problems existing in the above-mentioned prior art and provides a continuous homogeneous production device and a production method of acrylonitrile polymer for PAN carbon fiber precursor.

[0005] The above technical problems of the present invention are mainly solved by the following technical scheme: a continuous homogeneous production equipment of acrylonitrile polymer for PAN carbon fiber precursor, including a preparation tank, characterized in that: the output pipe of the preparation tank is respectively connected to a first polymerization kettle and a second polymerization kettle, and the two output ends of the output end pipes of the first polymerization kettle and the second polymerization kettle are connected to a polymer collection tank.

[0006] Preferably, a polymer discharge pump is provided on the output end of the polymer collection tank, a static mixer is connected to the pipeline at the output end of the polymer discharge pump, a de-singling tower is connected to the pipeline at the output end of the static mixer, a de-singling tower is connected to the output pipe of the de-singling tower liquid, a de-singling tower discharge pump is connected to the output pipe of the de-singling tower discharge pump, a raw liquid filter is arranged on the pipeline at the output end of the raw liquid filter, a degassing tower is connected to the pipeline at the output end of the degassing tower liquid, a polymer finished product tank is connected to the output pipe of the degassing tower, a degassing tower discharge pump is arranged on the pipeline between the degassing tower and the polymer finished product tank, a spinning liquid delivery pump is connected to the output pipe of the polymer finished product tank, and the spinning liquid delivery pump is connected to an external spinning unit.

[0007] Preferably, the output pipe of the de-singling tower gas is connected to a de-singling ejector, the output pipe of the de-singling ejector is connected to a first-level de-singling vacuum condenser, the pipeline at the output end of the first-level de-singling vacuum condenser is connected to two branch pipelines, and the two branch pipelines are respectively provided with a first de-singling liquid ring vacuum pump and a second de-singling liquid ring vacuum pump, the pipelines at the output ends of the first de-singling liquid ring vacuum pump and the second de-singling liquid ring vacuum pump are connected to a de-singling gas-liquid separator, the liquid condensed by the de-singling gas-liquid separator is connected to the inside of a second-level de-singling vacuum condenser through a pipeline, the condensate produced by the second-level de-singling vacuum condenser is again connected to the pipeline at the output end of the first-level de-singling vacuum condenser through a pipeline, and is circulated in and out again, and the gas in the de-singling gas-liquid separator is discharged through an external tail gas removal device.

[0008] Preferably, the output pipe of the debubbling tower gas is connected to a debubbling ejector, the output pipe of the debubbling ejector is connected to a first-level debubbling vacuum condenser, the pipe at the output end of the first-level debubbling vacuum condenser is connected to two branch pipes, and the two branch pipes are respectively provided with a first debubbling vacuum pump and a second debubbling vacuum pump, the pipes at the output ends of the first debubbling vacuum pump and the second debubbling vacuum pump are connected to a debubbling gas-liquid separator, the liquid condensed by the debubbling gas-liquid separator is connected to the inside of a second-level debubbling vacuum condenser through a pipe, the condensate produced by the second-level debubbling vacuum condenser is again connected to the pipe at the output end of the first-level debubbling vacuum condenser through a pipe, and is circulated in and out again, and the gas in the debubbling gas-liquid separator is discharged through an external tail gas removal device.

[0009] A method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor:

[0010] Step 1: Add 21.88% of acrylonitrile, 0.22% of methylene succinic acid, 0.27% of methyl acrylate and 77.37% of dimethyl sulfoxide into a preparation tank according to the weight ratio and stir.

[0011] Step 2: The polymerization reaction of the raw materials takes 14-16 hours. After stirring, the raw materials are injected into the first polymerization kettle below through a pipeline for polymerization for 7-8 hours. New raw materials are filled into the preparation tank and stirred, and then injected into the second polymerization kettle for polymerization for 7-8 hours. The first polymerization kettle and the second polymerization kettle react continuously with each other. When the first polymerization kettle and the second polymerization kettle react, it is necessary to fill 0.15% of azobisisobutyronitrile as an initiator and 0.11% of β-hydroxyethanethiol as a molecular weight regulator.

[0012] Step 3: After the first polymerization kettle has reacted for 14-16 hours, the polymer is sent to a polymer collection tank through a pipeline for storage. At the same time, the polymer in the second polymerization kettle is also sent to a polymer collection tank for storage after reacting for 14-16 hours.

[0013] Step 4: The polymer is sent to the degassing tower through a pipeline for degassing treatment, and then sent to the degassing tower for degassing treatment, and then discharged into the polymer finished product tank for storage, and finally discharged through the spinning solution delivery pump.

[0014] Preferably, the polymerization is started after maintaining at 60°C for 6 hours. After 8-10 hours, low-temperature chilled water is injected into the first polymerization kettle and the second polymerization kettle through pipelines to control the internal temperature at 70°C, and the double bonds are opened and connected to each other to form linear PAN macromolecular chains, releasing reaction heat to finally generate PAN.

[0015] Preferably, the initiator needs to be polymerized in the range of 55-65°C. At the same time, during the polymerization reaction, the temperature of the low-temperature cooling water filled into the first polymerization kettle and the second polymerization kettle through pipelines is controlled at: the supply water temperature is 5°C±5, and the return water temperature is controlled at 15°C±5.

[0016] Preferably, the top temperature of the de-monomerization tower is set to 75±5°C, the bottom temperature is set to 165±5°C, and the internal pressure is maintained at -150KPa(G). At the same time, 0.5MPa(G) saturated steam is fed into the bottom of the de-monomerization tower 7 at a flow rate of 240kg / h. The saturated steam removes the unreacted monomers from bottom to top, and a mixed gas composed of unreacted monomers and dimethyl sulfoxide vapor is obtained at the top of the de-monomerization tower. The gas is fed into the de-monomerization tower vacuum system on one side through a pipeline, and the polymer is fed into the degassing tower through the de-monomerization tower discharge pump and the raw liquid filter.

[0017] As a preference, the degassing tower is injected through a pipeline at a flow rate of 1 Nm 3 / h of ammonia, the gas produced is sent to the degassing tower vacuum system on one side through a pipeline, and the polymer produced is sent to the polymer finished product tank through the degassing tower discharge pump, and finally a polymer slurry with a molecular weight of 250,000-350,000 is obtained through a spinning liquid delivery pump, that is, polyacrylonitrile polymer for PAN carbon fiber precursor, and delivered to the spinning unit.

[0018] Preferably, a pipeline for injecting nitrogen is connected in the pipeline between the degassing tower and the degassing tower discharge pump, a two-stage vacuuming process is adopted in the degassing tower and the depolymerization tower, and the preparation tank, the first polymerization kettle, the second polymerization kettle and the polymer collection tank are all filled with nitrogen.

[0019] The present invention has the beneficial effects as follows: the present invention arranges a first polymerization kettle and a second polymerization kettle for uninterrupted polymerization reaction, so that a polymer requiring an extra-long polymerization reaction can be quickly produced again by the second polymerization kettle after being produced by controlling the first polymerization kettle, so that the time of the two is separated, thereby producing more polymers in a shorter time, so that the entire subsequent process can be operated uninterruptedly, reducing the time for shutdown and waiting, and reducing the energy consumption required for the second preheating of the equipment. At the same time, both the single removal tower and the degassing tower adopt a two-stage vacuuming process, which effectively ensures the vacuum degree and has a good single removal and degassing effect.

[0020] The solution polymerization mechanism initiated by azo free radicals is adopted, which has low production risk, high molecular weight of the polymerization product, low branching degree, and is not easy to produce gel and side reactions. Dimethyl sulfoxide has good solubility, is not easy to hydrolyze and has few side reactions, and is suitable for a variety of initiation systems. The initiation process of azobisisobutyronitrile is efficient and the speed is controllable. The polymerization temperature is between 60 and 70°C, and the production is safe and controllable. At the same time, the dilute dimethyl sulfoxide solution can be recycled repeatedly, has low toxicity, is not easy to volatilize, and the labor protection measures for operators are simple, and the investment in safety and environmental protection is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the equipment process structure of the present invention.

[0022] In the figure: 1, preparation tank; 2, first polymerization kettle; 3, second polymerization kettle; 4, polymer collecting tank; 5, polymer discharge pump; 6, static mixer; 7, degassing tower; 8, degassing tower discharge pump; 9, raw liquid filter; 10, degassing tower; 11, degassing tower discharge pump; 12, polymer finished product tank; 13, spinning liquid delivery pump; 14, degassing ejector; 15, primary degassing vacuum condenser; 16, first degassing liquid ring vacuum pump; 17, second degassing liquid ring vacuum pump; 18, degassing gas-liquid separator; 19, secondary degassing vacuum condenser; 20, degassing ejector; 21, primary degassing vacuum condenser; 22, first degassing vacuum pump; 23, second degassing vacuum pump; 24, degassing gas-liquid separator; 25, secondary degassing vacuum condenser. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further specifically described below through embodiments and in conjunction with the accompanying drawings.

[0024] Embodiment: A continuous homogeneous production device and method for producing acrylonitrile polymer for PAN carbon fiber precursor, such as Figure 1As shown, solvent and multiple monomers are put into the preparation tank 1 for stirring, the pipeline at the output end of the preparation tank 1 is respectively connected to the first polymerization kettle 2 and the second polymerization kettle 3, the output end pipelines of the first polymerization kettle 2 and the second polymerization kettle 3 are merged and connected to the polymer collection tank 4, the output end of the polymer collection tank 4 is connected to the depolymerization tower 7, the middle section of the output pipe of the polymer collection tank 4 is respectively provided with a polymer discharge pump 5 and a static mixer 6, the output pipe of the depolymerization tower 7 liquid is connected to the degassing tower 10, the pipeline between the depolymerization tower 7 and the degassing tower 10 is respectively connected to the depolymerization tower discharge pump 8 and the stock liquid filter 9, the stock liquid filter 9 adopts a 5-10μ disc type stock liquid filter 9, the output pipe of the degassing tower 10 liquid is connected to the polymer finished product tank 12, the pipeline between the degassing tower 10 and the polymer finished product tank 12 is provided with a degassing tower discharge pump 11, the output pipe of the polymer finished product tank 12 is connected to the spinning liquid delivery pump 13, and the spinning liquid delivery pump 13 is connected to the external spinning unit. The above are the preliminary equipment used in PAN production, and the corresponding steps are:

[0025] 1. The initiator and the molecular weight regulator are continuously fed into the preparation tank 1 at a certain flow rate, wherein the raw material components and flow rates of the monomers are as follows: 21.88% of the first monomer acrylonitrile, 0.22% of the second monomer methylene succinic acid, 0.27% of the third monomer methyl acrylate and 77.37% of dimethyl sulfoxide are injected per hour, and the above solvents are stirred inside the preparation tank 1. The first polymerization kettle 2 and the second polymerization kettle 3 are provided with a stirrer with variable frequency speed regulation. Under normal circumstances, the higher the speed, the lower the viscosity of the fluid, which further affects the molecular weight of PAN. In this application, the molecular weight of PAN is required to be 250,000 to 350,000, and the viscosity is 50 to 60 Pa.s as the best;

[0026] 2. The fused solution is respectively injected into the first polymerization kettle 2 and the second polymerization kettle 3. At the same time, the initiator 0.15% azobisisobutyronitrile and the molecular weight regulator 0.11% β-hydroxyethanethiol are respectively injected into the first polymerization kettle 2 and the second polymerization kettle 3 for reaction. The polymerization is started after maintaining at 60°C for 6 hours. After 10 hours, the internal temperature is controlled at 70°C by injecting low-temperature chilled water into the kettle through pipelines. The double bonds are opened and connected to each other as linear PAN macromolecular chains, releasing reaction heat, and finally generating PAN. The initiator needs to be polymerized in the range of 55-65°C. At the same time, during the polymerization reaction, the low-temperature cooling water filled into the first polymerization kettle 2 and the second polymerization kettle 3 through the pipeline is controlled at the following temperature: the water supply temperature is 5°C ± 5, and the return water temperature is controlled at 15°C ± 5 (low temperature The cooling water is based on the heat release of acrylonitrile polymerization of 72KJ / mol, and the heat release of polymerization matching 10000t / a raw silk is 1840000KJ / mol, and the low-temperature freezing water consumption is 88t / h). The above working sequence is: first put it into the first polymerization kettle 2 for reaction for 7-8h, then put the raw materials in step 1 again for stirring and then send them into the second polymerization kettle 3 for reaction, and then wait for the second polymerization kettle 3 to react again for 7-8h. At this time, the polymer in the first polymerization kettle 2 has been reacted for 14-16h and the required PAN is produced. At this time, it can be injected into the polymer collection tank 4 below. At this time, new raw materials can be added to the first polymerization kettle 2. After reacting for 7-8h, the second polymerization kettle 3 can be discharged. The reciprocating reaction ensures that there is always PAN in the polymer collection tank 4.

[0027] 3. The polymer after final polymerization flows into the polymer collecting tank 4, and then flows into the depolymerizing tower 7 through the polymer discharging pump 5 and the static mixer 6. The static mixer 6 is used to change the flow state of the fluid so as to achieve good dispersion and sufficient mixing between different fluids. Jackets are set on the outside of the preparation tank 1, the first polymerization kettle 2, the second polymerization kettle 3 and the polymer collecting tank 4. The jacket on the outside of the preparation tank 1 is filled with jacket water of 25°C, the jackets on the outer surfaces of the first polymerization kettle 2 and the second polymerization kettle 3 are filled with jacket water of 5°C±5, and the jacket on the outer surface of the polymer collecting tank 4 is filled with jacket water of 45°C and 80°C respectively. The water of different temperatures can be replaced at any time according to the different temperatures of the internal tank body. At the same time, 0.5MPa (G) saturated steam is fed into the bottom of the de-monomerization tower 7 at a flow rate of 240kg / h. The saturated steam removes the unreacted monomers from bottom to top. A mixed gas consisting of unreacted monomers and dimethyl sulfoxide vapor is obtained at the top of the de-monomerization tower 7, which is fed into the de-monomerization ejector 14 for vacuuming, and then fed into the vacuum system of the de-monomerization tower 7 for circulation. The polymer at the bottom of the tower is fed into the 5-10μ disc-type raw liquid filter 9 through the bottom pump 8 of the de-monomerization tower 7 to filter out large polymers, and then the polymer is transported to the degassing tower 10.

[0028] 4. Ammonia is injected into the polymer at the bottom of degassing tower 10, with a flow rate of 1Nm 3 / h, the purpose is to improve the hydrophilicity of the resin. Homopolymer PAN is hydrophobic, and the hydrophobicity of copolymer PAN has changed, but it is still a hydrophobic system. After amination, 20% of the carboxyl groups are replaced by carboxyl ammonium to generate β-ammonium itaconate. The introduction of PAN macromolecular chains can significantly improve the hydrophilicity and significantly reduce the contact angle with water. The polymer is transported to the polymer finished product tank 12 through the degassing tower discharge pump 11, and is transported to the spinning liquid delivery pump (13) to obtain a polymer slurry with a molecular weight of 250,000-350,000, that is, a polyacrylonitrile polymer for PAN carbon fiber precursor, and finally transported to an external spinning unit. At the same time, the mixed gas generated in the degassing tower 10 flows into the vacuum system of the degassing tower 10 through the degassing ejector 20 on one side to circulate.

[0029] The vacuum system of the stripping tower 7 includes:

[0030] The output pipe of the gas from the de-singling tower 7 is connected to a de-singling ejector 14, and the mixed gas obtained through the de-singling tower 7 is sent to the de-singling ejector 14 through the gas outlet at the top of the de-singling tower 7. The gas is sent to the first-stage de-singling vacuum condenser 15 through the output pipe of the de-singling ejector 14, and then enters the first de-singling liquid ring vacuum pump 16 for further vacuuming. Two branch pipes are connected to the pipe at the output end of the first-stage de-singling vacuum condenser 15, and the first de-singling liquid ring vacuum pump 16 and the second de-singling liquid ring vacuum pump 17 are respectively provided on the two branch pipes. The second de-singling liquid ring vacuum pump 17 is a backup pump for the first de-singling liquid ring vacuum pump 16, and the first de-singling liquid ring vacuum pump 16 is a backup pump for the first de-singling liquid ring vacuum pump 16. The pipelines at the output ends of the ring vacuum pump 16 and the second de-singling liquid ring vacuum pump 17 are connected to the de-singling gas-liquid separator 18. The de-singling gas-liquid separator 18 condenses the gas into liquid and transports it to the inside of the second-stage de-singling vacuum condenser 19 through a pipeline. The condensate produced by the second-stage de-singling vacuum condenser 19 is again sent to the pipeline at the output end of the first-stage de-singling vacuum condenser 15 through a pipeline to circulate again. The gas in the de-singling gas-liquid separator 18 is discharged through an external tail gas removal device. The top temperature of the de-singling tower 7 is set to 75±5℃, the bottom temperature is set to 165±5℃, and the internal pressure is maintained at -150KPa(G).

[0031] The vacuum system of the degassing tower 10 includes:

[0032] The gas output pipe of the degassing tower 10 is connected to the degassing ejector 20, and the mixed gas obtained by the degassing tower 10 is sent to the degassing ejector 20 through the gas outlet at the top of the tower. The gas is sent to the primary degassing vacuum condenser 21 through the output pipe of the degassing ejector 20, and then further evacuated by the first degassing vacuum pump 22. Two branch pipes are connected to the pipe at the output end of the primary degassing vacuum condenser 21, and the first degassing vacuum pump 22 and the second degassing vacuum pump 23 are respectively provided on the two branch pipes. 22 is a backup pump for the first degassing vacuum pump 22. The pipelines at the output ends of the first degassing vacuum pump 22 and the second degassing vacuum pump 23 are connected to a degassing gas-liquid separator 24. The degassing gas-liquid separator 24 condenses the gas into liquid and sends it to the inside of the secondary degassing vacuum condenser 25 through a pipeline. The condensate produced by the secondary degassing vacuum condenser 25 is sent to the pipeline at the output end of the primary degassing vacuum condenser 21 through a pipeline for recirculation. The gas in the degassing gas-liquid separator 24 is discharged through an external exhaust device. Tables 1 and 2 are actual comparisons of the overall energy consumption of the original process and the current process:

[0033] Table 1

[0034]

[0035] Table 2

[0036]

[0037] Table 3 compares the continuous polymerization of PAN-based carbon fiber homogeneous solution of the present invention with the intermittent polymerization of conventional PAN-based carbon fiber homogeneous solution:

[0038] Table 3

[0039]

[0040] Table 4 is a data comparison of the specific stirring speeds of the variable frequency speed regulating stirrers in the first polymerization kettle and the second polymerization kettle:

[0041] Serial number Speed ​​(rpm) Molecular weight Viscosity(Pa.s) 1 30~35 200,000-250,000 40~50 2 35~40 250,000-350,000 50~60 3 40~45 350,000-400,000 60~70

[0042] Table 5 shows the calculation of the acrylonitrile polymerization system of the present invention based on 10000t / a raw yarn. The main equipment structure and dimensions of the polymerization unit are shown in the following table:

[0043]

[0044]

[0045] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention should be considered to belong to the protection scope of the present invention.

Claims

1. A continuous homogeneous production device for acrylonitrile polymer for PAN carbon fiber precursor, comprising a preparation tank (1), characterized in that: The output pipeline of the preparation tank (1) is respectively connected to the first polymerization kettle (2) and the second polymerization kettle (3), and the two output ends of the output end pipelines of the first polymerization kettle (2) and the second polymerization kettle (3) are connected to a polymer collection tank (4).

2. The continuous homogeneous production equipment of acrylonitrile polymer for PAN carbon fiber precursor according to claim 1, characterized in that: A polymer discharge pump (5) is provided on the output end of the polymer collection tank (4); a static mixer (6) is connected to the pipeline at the output end of the polymer discharge pump (5); a depolymerization tower (7) is connected to the pipeline at the output end of the static mixer (6); a depolymerization tower discharge pump (8) is connected to the output pipe of the depolymerization tower (7); a raw liquid filter (9) is provided on the pipeline at the output end of the depolymerization tower discharge pump (8); a degassing tower (10) is connected to the pipeline at the output end of the raw liquid filter (9); a polymer finished product tank (12) is connected to the output pipe of the degassing tower (10); a degassing tower discharge pump (11) is provided on the pipeline between the degassing tower (10) and the polymer finished product tank (12); a spinning liquid delivery pump (13) is connected to the output pipe of the polymer finished product tank (12); and the spinning liquid delivery pump (13) is connected to an external spinning unit.

3. The continuous homogeneous production equipment of acrylonitrile polymer for PAN carbon fiber precursor according to claim 2, characterized in that: The output pipe of the gas from the de-singling tower (7) is connected to a de-singling ejector (14), and the output pipe of the de-singling ejector (14) is connected to a first-stage de-singling vacuum condenser (15). The pipeline at the output end of the first-stage de-singling vacuum condenser (15) is connected to two branch pipelines, and the two branch pipelines are respectively provided with a first de-singling liquid ring vacuum pump (16) and a second de-singling liquid ring vacuum pump (17). The pipelines at the output ends of the first de-singling liquid ring vacuum pump (16) and the second de-singling liquid ring vacuum pump (17) are connected to a de-singling gas-liquid separator (18). The liquid condensed by the de-singling gas-liquid separator (18) is connected to a second-stage de-singling vacuum condenser (19) through a pipeline. The condensate generated by the second-stage de-singling vacuum condenser (19) is again connected to the pipeline at the output end of the first-stage de-singling vacuum condenser (15) through a pipeline and enters and exits for re-circulation. The gas in the de-singling gas-liquid separator (18) is discharged through an external tail gas removal device.

4. The continuous homogeneous production equipment of acrylonitrile polymer for PAN carbon fiber precursor according to claim 2, characterized in that: The gas output pipe of the degassing tower (10) is connected to a degassing ejector (20), and the output pipe of the degassing ejector (20) is connected to a primary degassing vacuum condenser (21). The pipeline at the output end of the primary degassing vacuum condenser (21) is connected to two branch pipelines, and the two branch pipelines are respectively provided with a first degassing vacuum pump (22) and a second degassing vacuum pump (23). The pipelines at the output ends of the first degassing vacuum pump (22) and the second degassing vacuum pump (23) are connected to a degassing gas-liquid separator (24). The liquid condensed by the degassing gas-liquid separator (24) is connected to the inside of a secondary degassing vacuum condenser (25) through a pipeline. The condensate generated by the secondary degassing vacuum condenser (25) is again connected to the pipeline at the output end of the primary degassing vacuum condenser (21) through a pipeline, and is circulated in and out again. The gas in the degassing gas-liquid separator (24) is discharged through an external tail gas removal device.

5. A method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor, the steps comprising: Step 1: Add 21.88% of acrylonitrile as the first monomer, 0.22% of methylene succinic acid as the second monomer, 0.27% of methyl acrylate as the third monomer and 77.37% of dimethyl sulfoxide as the solvent into a preparation tank (1) according to the weight ratio and stir. Step 2: The polymerization reaction of the raw materials takes 14-16 hours. After stirring, the raw materials are injected into the first polymerization kettle (2) below through a pipeline for polymerization for 7-8 hours. Then, new raw materials are added to the preparation tank (1) and stirred, and then injected into the second polymerization kettle (3) for polymerization for 7-8 hours. The first polymerization kettle (2) and the second polymerization kettle (3) react continuously with each other. When the first polymerization kettle (2) and the second polymerization kettle (3) react, 0.15% of azobisisobutyronitrile as an initiator and 0.11% of β-hydroxyethanethiol as a molecular weight regulator need to be added. Step 3: After the first polymerization kettle (2) has reacted for 14-16 hours, the polymer is sent to the polymer collection tank (4) through a pipeline for storage. At the same time, the polymer in the second polymerization kettle (3) is also sent to the polymer collection tank (4) for storage after reacting for 14-16 hours. Step 4: The polymer is sent to the degassing tower (7) through a pipeline for degassing, and then sent to the degassing tower (10) for degassing, and then discharged into the polymer finished product tank (12) for storage, and finally discharged through the spinning solution delivery pump (13).

6. The method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor according to claim 5, wherein step 2 comprises: After maintaining the temperature at 60°C for 6 hours, polymerization begins. After 8-10 hours, low-temperature chilled water is injected into the first polymerization kettle (2) and the second polymerization kettle (3) through pipelines to control the internal temperature at 70°C. Double bonds are opened and connected to each other to form linear PAN macromolecular chains, releasing reaction heat to eventually generate PAN.

7. The method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor according to claim 6, wherein step 2 comprises: The initiator needs to polymerize within the range of 55-65°C. At the same time, during the polymerization reaction, the temperature of the low-temperature cooling water filled into the first polymerization kettle (2) and the second polymerization kettle (3) through pipelines is controlled at: the supply water temperature is 5°C±5, and the return water temperature is controlled at 15°C±5.

8. The method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor according to claim 5, wherein step 4 comprises: The top temperature of the de-monomer tower (7) is set to 75±5°C, the bottom temperature is set to 165±5°C, and the internal pressure is maintained at -150KPa(G). At the same time, 0.5MPa(G) saturated steam is fed into the bottom of the de-monomer tower (7) at a flow rate of 240kg / h. The saturated steam removes the unreacted monomers from bottom to top, and a mixed gas composed of unreacted monomers and dimethyl sulfoxide vapor is obtained at the top of the de-monomer tower (7). The gas is fed into the vacuum system of the de-monomer tower (7) on one side through a pipeline, and the polymer is fed into the interior of the degassing tower (10) through the de-monomer tower discharge pump (8) and the raw liquid filter (9).

9. The method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor according to claim 5, wherein step 4 comprises: The flow rate of the degassing tower (10) injected through the pipeline is 1Nm 3 / h of ammonia, the gas produced is sent to the vacuum system of a degassing tower (10) on one side through a pipeline, and the polymer produced is sent to a polymer finished product tank (12) through a degassing tower discharge pump (11), and finally a polymer slurry with a molecular weight of 250,000 to 350,000 is obtained through a spinning liquid delivery pump (13), that is, a polyacrylonitrile polymer for PAN carbon fiber precursor, and is delivered to a spinning unit.

10. The method for producing a continuous homogeneous phase of acrylonitrile polymer for PAN carbon fiber precursor according to claim 5, wherein step 4 comprises: A pipeline for injecting nitrogen is connected to the pipeline between the degassing tower (10) and the degassing tower discharge pump (11); a two-stage vacuum pumping process is adopted in the degassing tower (10) and the desing tower (7); and the preparation tank (1), the first polymerization kettle (2), the second polymerization kettle (3) and the polymer collection tank (4) are all filled with nitrogen.