Preparation method of morphology-controllable palladium-tin intermetallic compound

The palladium-tin intermetallic compounds prepared by high-temperature pyrolysis and modified soybean phospholipids were solved, and the catalytic performance and stability of single-metal nanoenzyme materials were insufficient, the morphology of bimetallic nanoenzyme materials was uncontrollable, and the palladium-tin nanoenzymes were insoluble in water. Problem, the preparation of palladium-tin intermetallic compound catalyst with controllable morphology and good stability has been achieved, and is suitable for biomedical and diagnostic fields.

CN118904331AActive Publication Date: 2024-11-08HARBIN ENG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410943250.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The catalytic performance and stability of existing single-metal nanoenzyme materials are poor, the preparation of bimetal nanoenzyme materials is uncontrollable, and common palladium-tin nanoenzyme catalysts are insoluble in water.

Method used

The high-temperature pyrolysis method is used to prepare palladium-tin intermetallic compounds with controllable morphology. By controlling the mass ratio of methylamine hydrochloride and tin acetate, the reaction is carried out under high temperature conditions to produce palladium-tin intermetallic compounds with different morphology, and soybeans are carried out. Phospholipids are modified to improve their water solubility and stability.

Benefits of technology

Prepare a palladium-tin intermetallic compound bimetallic nanoenzyme catalyst with controllable morphology and size. It has good catalytic performance and stability, excellent near-infrared light absorption capacity and catalytic activities of multiple enzymes. It is suitable for nanobiomedicine research field , and tin ions in palladium-tin intermetallic compounds have a high X-ray attenuation coefficient, which is suitable for disease diagnosis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904331A_ABST
    Figure CN118904331A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a palladium-tin intermetallic compound, in particular to a preparation method of a morphology-controllable palladium-tin intermetallic compound. The invention aims to solve the problems that the existing monometal nano-enzyme material is poor in catalytic performance and stability and single in enzyme activity; the problems that an existing bimetallic nano-enzyme material is uncontrollable in preparation morphology, and a common palladium-tin nano-enzyme catalyst is insoluble in water are solved. The preparation comprises the following steps: preparing a palladium-tin intermetallic compound by a high-temperature pyrolysis method; and 2, surface modification of the palladium-tin intermetallic compound. The method is used for preparing the palladium-tin intermetallic compound with the controllable morphology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a palladium-tin intermetallic compound. Background Art

[0002] Nanozyme catalysts can be used as substitutes for natural enzymes due to their advantages such as high surface area ratio, enzyme activity and good biocompatibility. Breakthroughs have been made in the fields of clinical medicine, food safety, environmental monitoring and chemical production, especially in the fields of bioanalysis, antibacterial, anti-inflammatory and anti-cancer. In the field of bioanalysis, colorimetry, electrochemical methods, enzyme-linked immunosorbent assays based on nanozymes are used to improve the sensitivity and specificity of detection of various substances (heavy metal ions, biomarkers, pathogenic microorganisms, antibodies, etc.).

[0003] Existing nanozyme catalysts are often composed of carbon-based materials, metals, and transition metal compounds. In general, the structural characteristics of existing metal and metal oxide-based nanozymes can be roughly divided into single metals, metal alloys, metal oxides, metal core / shell nanostructures, and hybrid nanomaterials. Due to their excellent physicochemical properties (such as high surface energy, superior optical and photothermal conversion properties), metal and metal oxide-based nanozymes have the characteristics of low cost, high stability, and easy storage, which has important guiding significance for in-depth research on their catalytic activity and mechanism.

[0004] Single metal nanozymes are usually precious metal nanomaterials with significant chemical stability under natural conditions. They usually have sites that are easily coupled with a variety of biomolecular ligands and antibodies, significant surface plasmon resonance (SPR) properties, and superior optical and photothermal conversion properties. However, bare single metal nanoparticles (such as Ag, Pt) have a single active site and are not suitable for complex catalytic reactions. At the same time, single metal nanozymes are easy to sinter at high temperatures, are easily competitively adsorbed by poisons, and have poor resistance to CO2 and SO2 (i.e., the catalytic activity is significantly reduced in the presence of CO2 or SO2), and they are easy to aggregate into nanoclusters, resulting in reduced catalytic activity. Most importantly, most bare precious metal nanozymes (except gold) are biologically toxic, which limits their application in clinical medicine.

[0005] The adjacent bimetallic atoms in the bimetallic nanozyme catalyst provide co-adsorption sites for molecules, which is beneficial to the activation of molecules by stretching chemical bonds or adjusting the adsorption layout. The strong interaction between bimetallic atoms helps to regulate the electronic structure and promote the adsorption / desorption of intermediates. At the same time, there is a synergistic effect between bimetallic atoms, which is conducive to the efficient catalysis of complex reactions. When the bimetallic nanozyme catalyst is catalytic, it produces less CO2 and has higher tolerance to CO2. Compared with metal nanoparticles, bimetallic nanoparticles have lower biological activity. At the same time, bimetallic nanoparticles are generally not genotoxic, which makes them safer to use. However, due to the complexity of the structure of bimetallic nanozyme catalysts, there is often structural heterogeneity and uncontrollable preparation morphology, and common palladium tin nanozyme catalysts are insoluble in water. Summary of the invention

[0006] The present invention aims to solve the problems that the existing single-metal nanozyme materials have poor catalytic performance and stability, and single enzyme activity; solve the problems that the morphology of the existing bimetallic nanozyme materials is uncontrollable, and the common palladium-tin nanozyme catalyst is insoluble in water, and further provide a method for preparing a palladium-tin intermetallic compound with controllable morphology.

[0007] A method for preparing a palladium-tin intermetallic compound with controllable morphology is carried out according to the following steps:

[0008] 1. Preparation of palladium-tin intermetallic compounds by high temperature pyrolysis:

[0009] Under magnetic stirring conditions, oleylamine, methylamine hydrochloride, acetylacetonate palladium and tin acetate are uniformly mixed to obtain a mixed solution A; under a vacuum state, the mixed solution A is heated to 40°C to 45°C, and kept warm for 20min to 25min at a temperature of 40°C to 45°C, the vacuum device is closed, nitrogen is introduced, and the temperature is kept at 55°C to 60°C for 30min to 35min to form a uniform solution, trioctylphosphine is added to the uniform solution, and the temperature is kept at 200°C to 210°C for 30min to 35min to obtain a mixed solution B, the mixed solution B is heated to 300°C to 310°C, and the temperature is 300°C to 310°C for 25min to 30min, and after the reaction is completed, the mixed solution is naturally cooled to room temperature, and the solution is collected by centrifugation and washed to obtain a palladium-tin intermetallic compound;

[0010] When the mass ratio of methylamine hydrochloride to tin acetate is (0-0.25):1, the palladium-tin intermetallic compound is a nanodot with a particle size of 5nm-10nm;

[0011] When the mass ratio of methylamine hydrochloride to tin acetate is (0.5-0.75):1, the palladium-tin intermetallic compound is a nanorod with a length of 30 nm to 35 nm;

[0012] When the mass ratio of methylamine hydrochloride to tin acetate is (1.25-1.5):1, the palladium-tin intermetallic compound is a nanorod with a length of 70 nm to 75 nm;

[0013] When the mass ratio of methylamine hydrochloride to tin acetate is (2.5-2.75):1, the palladium-tin intermetallic compound is a nanorod with a length of 120 nm to 125 nm;

[0014] 2. Surface modification of palladium-tin intermetallic compounds:

[0015] The palladium-tin metal compound is dissolved in cyclohexane, and then a chloroform solution of soybean lecithin is added dropwise, and the solvent is evaporated in a rotary evaporator under vacuum at a temperature of 60° C. to obtain the palladium-tin metal compound modified with soybean lecithin.

[0016] The beneficial effects of the present invention are:

[0017] ①. The present invention prepares a palladium-tin intermetallic compound bimetallic nanozyme catalyst with controllable morphology and size, which has good catalytic performance and stability.

[0018] ②. The material is obtained in one step by high-temperature pyrolysis method, with palladium acetylacetonate as the palladium source and tin acetate as the tin source. By controlling the amount of methylamine hydrochloride, a palladium-tin intermetallic compound with controllable morphology is generated under high temperature conditions.

[0019] ③. Characterization experiments and density functional theory calculation results have confirmed that the ordered palladium-tin intermetallic compounds have excellent near-infrared light absorption and multiple enzyme catalytic activities (such as catalase, peroxidase and oxidase-like activity). Comparative experiments have found that nanorods with higher specific surface areas have better performance. Therefore, palladium-tin intermetallic compounds with controllable morphology are expected to be applied in the field of nanobiomedical research.

[0020] ④. The tin ions in palladium-tin intermetallic compounds have a high X-ray attenuation coefficient and can be used as contrast agents for computed tomography imaging, for disease diagnosis and real-time monitoring of treatment processes.

[0021] Therefore, the morphology-controllable palladium-tin intermetallic compound involved in the present invention has controllable morphology, good stability and catalytic performance, and good photothermal and optical properties.

[0022] Instruction Manual

[0023] Figure 1 This is a diagram of the synthesis process of preparing a soybean lecithin-modified palladium-tin intermetallic compound according to Example 1;

[0024] Figure 2TEM images and elemental mapping images of Pd2Sn NDs and Pd2SnNRs prepared in step 1 of Example 1 at different magnifications;

[0025] Figure 3 TEM images and elemental mapping images of Pd2Sn SNRs and Pd2Sn LNRs prepared in step 1 of Example 1 at different magnifications;

[0026] Figure 4 High-resolution transmission electron microscopy images and lattice spacing measurements of Pd2SnNRs and Pd2Sn NDs prepared in step 1 of Example 1;

[0027] Figure 5 The EDS measurement spectrum of Pd2SnNRs prepared in step 1 of Example 1;

[0028] Figure 6 PXRD images of Pd2Sn NDs, Pd2Sn SNRs, Pd2Sn NRs and Pd2Sn LNRs prepared in step 1 of Example 1, a is Pd2Sn NRs and Pd2Sn NDs, b is a local enlarged view of a, and c is Pd2Sn LNRs and Pd2Sn SNRs;

[0029] Figure 7 The XPS measurement spectra of Pd2SnNRs and Pd2SnNDs prepared in step 1 of Example 1;

[0030] Figure 8 High-resolution XPS measurement spectra of Pd 3d and Sn 3d energy levels of Pd2SnNRs and Pd2SnNDs prepared in step 1 of Example 1;

[0031] Fig. 9 The photothermal stability test diagram of Pd2Sn-SPNRs aqueous solution, a is the photothermal conversion efficiency, b is the change of hot and cold cycle temperature;

[0032] Fig.10 1 is the fitting curve of the mass extinction coefficient of the palladium-tin intermetallic compound modified with soybean lecithin prepared in Example 1, 1 is Pd2Sn-SPNRs, 2 is Pd2Sn-SPNDs;

[0033] Fig.11 The zeta potential of the Pd2Sn NRs prepared in step 1 of Example 1 and the Pd2Sn-SPNRs prepared in step 2;

[0034] Fig.12UV-vis-NIR absorption spectra of Pd2Sn-SPNRs aqueous solution and Pd2Sn-SPNDs aqueous solution, 1 is the concentration of 400μg / mL, 2 is the concentration of 300μg / mL, 3 is the concentration of 200μg / mL, 4 is the concentration of 100μg / mL, 5 is the concentration of 50μg / mL, and 6 is the concentration of 25μg / mL;

[0035] Fig.13 This is the ESR image of Pd2Sn-SPNRs prepared in Example 1, a is the detection 1 O2, b is detection of OH;

[0036] Fig.14 The UV-visible absorption spectra of the Pd2Sn-SPNRs prepared in Example 1 under different conditions for catalytic oxidation of OPD and TMB, a is OPD, b is TMB, 1 is Pd2Sn-SPNRs+hydrogen peroxide+laser irradiation, 2 is Pd2Sn-SPNRs+hydrogen peroxide, 3 is the laser irradiation group alone, and 4 is the control group;

[0037] Fig.15 The Michaelis-Menten kinetic analysis images and Lineweaver-Burk peroxidase simulation activity images of Pd2Sn-SP LNRs, Pd2Sn-SPNRs, Pd2Sn-SP SNRs and Pd2Sn-SPNDs prepared in Example 1, a is the Michaelis-Menten diagram, b is the Lineweaver-Burk diagram, 1 is Pd2Sn-SP LNRs, 2 is Pd2Sn-SPNRs, 3 is Pd2Sn-SP SNRs, and 4 is Pd2Sn-SPNDs;

[0038] Fig.16 The oxidase-like enzyme simulation activity of Pd2Sn-SP NRs prepared in Example 1 at different times, 1 is 10 min, 2 is 8 min, 3 is 6 min, 4 is 4 min, and 5 is 2 min;

[0039] Fig.17 The images of the degradation of methylene blue (MB) catalyzed by Pd2Sn-SPNRs prepared in Example 1 at different time points, 1 is 0 min, 2 is 2 min, 3 is 4 min, 4 is 6 min, 5 is 8 min, and 6 is 10 min;

[0040] Fig.18 The Pd2Sn-SPNRs prepared in Example 1 were illuminated at different concentrations and 808 nm laser (0.8 W / cm 2) Catalase-like activity under irradiation conditions, a is the catalase activity of Pd2Sn-SPNRs at different concentrations, 1 is 400μg / mL, 2 is 200μg / mL, 3 is 100μg / mL, 4 is 50μg / mL, 5 is pure water, b is the effect of laser irradiation on the catalase-like activity of Pd2Sn-SPNRs, 1 is 200μg / mL, 2 is 200μg / mL+808nm laser irradiation;

[0041] Fig.19 The palladium-tin intermetallic compounds of different morphologies prepared in Example 1 produce catalase-like activity under laser irradiation, 1 is 400 μg / mL, 2 is 200 μg / mL, 3 is 100 μg / mL, 4 is 50 μg / mL, and 5 is pure water;

[0042] Fig. 20 Effects of the Pd2Sn-SPNRs prepared in Example 1 on cell activity when co-incubated with normal cells (L929 cells) at different concentrations for 12 h and 24 h. DETAILED DESCRIPTION

[0043] Specific implementation method 1: This implementation method is a method for preparing a palladium-tin intermetallic compound with controllable morphology, which is carried out according to the following steps:

[0044] 1. Preparation of palladium-tin intermetallic compounds by high temperature pyrolysis:

[0045] Under magnetic stirring conditions, oleylamine, methylamine hydrochloride, acetylacetonate palladium and tin acetate are uniformly mixed to obtain a mixed solution A; under a vacuum state, the mixed solution A is heated to 40°C to 45°C, and kept warm for 20min to 25min at a temperature of 40°C to 45°C, the vacuum device is closed, nitrogen is introduced, and the temperature is kept at 55°C to 60°C for 30min to 35min to form a uniform solution, trioctylphosphine is added to the uniform solution, and the temperature is kept at 200°C to 210°C for 30min to 35min to obtain a mixed solution B, the mixed solution B is heated to 300°C to 310°C, and the temperature is 300°C to 310°C for 25min to 30min, and after the reaction is completed, the mixed solution is naturally cooled to room temperature, and the solution is collected by centrifugation and washed to obtain a palladium-tin intermetallic compound;

[0046] When the mass ratio of methylamine hydrochloride to tin acetate is (0-0.25):1, the palladium-tin intermetallic compound is a nanodot with a particle size of 5 nm to 10 nm;

[0047] When the mass ratio of methylamine hydrochloride to tin acetate is (0.5-0.75):1, the palladium-tin intermetallic compound is a nanorod with a length of 30 nm to 35 nm;

[0048] When the mass ratio of methylamine hydrochloride to tin acetate is (1.25-1.5):1, the palladium-tin intermetallic compound is a nanorod with a length of 70 nm to 75 nm;

[0049] When the mass ratio of methylamine hydrochloride to tin acetate is (2.5-2.75):1, the palladium-tin intermetallic compound is a nanorod with a length of 120 nm to 125 nm;

[0050] 2. Surface modification of palladium-tin intermetallic compounds:

[0051] The palladium-tin metal compound is dissolved in cyclohexane, and then a chloroform solution of soybean lecithin is added dropwise, and the solvent is evaporated in a rotary evaporator under vacuum at a temperature of 60° C. to obtain the palladium-tin metal compound modified with soybean lecithin.

[0052] In this embodiment, the metal palladium has multiple oxidation states and has good ability to absorb and transmit hydrogen, thus having good catalytic performance and multiple enzyme catalytic abilities. By adding tin to palladium to form a palladium-tin metal compound bimetallic catalyst, the ESR image of the material under laser irradiation is observed to evaluate the 1 The generation of O2 and ·OH is verified by testing its UV-vis-NIR absorption spectrum in an environment containing hydrogen peroxide, verifying the significant characteristic absorption of oxOPD (420nm) or oxTMB (652nm), methylene blue and its ability to exhibit good multi-enzyme catalytic ability (having catalase, peroxidase and oxidase-like activity). At the same time, its good catalytic ability can be verified by measuring its maximum reaction rate (Vmax) and Michaelis-Menten constant (Km). Experiments have proved that its catalytic ability can be further enhanced under laser irradiation, and its biological toxicity is low.

[0053] The beneficial effects of this embodiment are:

[0054] ①. This embodiment prepares a palladium-tin intermetallic compound bimetallic nanozyme catalyst with controllable morphology and size, which has good catalytic performance and stability.

[0055] ②. The material is obtained in one step by high-temperature pyrolysis method, with palladium acetylacetonate as the palladium source and tin acetate as the tin source. By controlling the amount of methylamine hydrochloride, a palladium-tin intermetallic compound with controllable morphology is generated under high temperature conditions.

[0056] ③. Characterization experiments and density functional theory calculation results have confirmed that the ordered palladium-tin intermetallic compounds have excellent near-infrared light absorption and multiple enzyme catalytic activities (such as catalase, peroxidase and oxidase-like activity). Comparative experiments have found that nanorods with higher specific surface areas have better performance. Therefore, palladium-tin intermetallic compounds with controllable morphology are expected to be applied in the field of nanobiomedical research.

[0057] ④. The tin ions in palladium-tin intermetallic compounds have a high X-ray attenuation coefficient and can be used as contrast agents for computed tomography imaging, for disease diagnosis and real-time monitoring of treatment processes.

[0058] Therefore, the morphology-controllable palladium-tin intermetallic compound involved in this embodiment has controllable morphology, good stability and catalytic performance, and good photothermal and optical properties.

[0059] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the mass ratio of oleylamine to tin acetate in step 1 is (0.30-0.35):1; the mass ratio of palladium acetylacetonate to tin acetate in step 1 is (1.70-1.75):1. The rest is the same as specific embodiment 1.

[0060] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the mass ratio of trioctylphosphine to tin acetate in step 1 is (0.30-0.35): 1. The rest is the same as specific embodiment 1 or 2.

[0061] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 1, oleylamine, methylamine hydrochloride, palladium acetylacetonate and tin acetate are mixed at a rotation speed of 500 rpm to 600 rpm for 5 min to 10 min to obtain a mixed solution A. The rest is the same as specific embodiments 1 to 3.

[0062] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: in step 1, the mixed solution A is heated to 40° C. to 45° C. at a heating rate of 2° C. / min to 3° C. / min. The rest is the same as specific embodiments 1 to 4.

[0063] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: in step 1, the mixed solution B is heated to 300° C. to 310° C. at a heating rate of 2° C. / min to 3° C. / min. The rest is the same as specific embodiments 1 to 5.

[0064] Specific embodiment 7: This embodiment is different from Specific embodiments 1 to 6 in that the washing in step 1 is washing with ethanol and chloroform alternately. The rest is the same as Specific embodiments 1 to 6.

[0065] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the mass ratio of cyclohexane to the palladium-tin intermetallic compound in step 2 is (790-795): 1. The rest is the same as specific embodiments 1 to 7.

[0066] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that the mass ratio of soybean lecithin to palladium-tin intermetallic compound in the chloroform solution of soybean lecithin described in step 2 is (6.0-6.5): 1. The rest is the same as specific embodiments 1 to 8.

[0067] Specific embodiment 10: This embodiment differs from Specific embodiments 1 to 9 in that the concentration of soybean lecithin in the chloroform solution of soybean lecithin in step 2 is 1 mg / mL to 1.5 mg / mL. The rest is the same as Specific embodiments 1 to 9.

[0068] The following examples are used to verify the beneficial effects of the present invention:

[0069] Embodiment 1, combined with Figure 1 Specific instructions:

[0070] A method for preparing a morphology-controllable palladium-tin intermetallic compound is carried out according to the following steps:

[0071] 1. Preparation of palladium-tin intermetallic compounds by high temperature pyrolysis:

[0072] At a rotation speed of 500 rpm, oleylamine, methylamine hydrochloride, acetylacetonate palladium (Pd(acac)2) and tin acetate (Sn(OAc)2) are mixed for 10 minutes to obtain a mixed solution A; under a vacuum state, the mixed solution A is heated to 40°C at a heating rate of 2°C / min, and is kept warm for 20 minutes at 40°C, the vacuum device is closed, nitrogen is introduced, and the temperature is kept warm for 30 minutes at 60°C to form a uniform solution, trioctylphosphine is added to the uniform solution, and the temperature is kept warm for 30 minutes at 200°C to obtain a mixed solution B; the mixed solution B is heated to 300°C at a heating rate of 2°C / min, and is reacted at 300°C for 30 minutes, and after the reaction is completed, it is naturally cooled to room temperature, collected by centrifugation, and washed alternately with ethanol and chloroform to obtain a palladium-tin intermetallic compound;

[0073] The mass ratio of oleylamine to tin acetate is 0.305:1; the mass ratio of palladium acetylacetonate to tin acetate is 1.717:1; the mass ratio of trioctylphosphine to tin acetate is 0.30:1;

[0074] When the mass ratio of methylamine hydrochloride to tin acetate is 0:1, the palladium-tin intermetallic compound is palladium-tin intermetallic compound nanodots (Pd2SnNDs) with a particle size of 5 nm to 10 nm;

[0075] When the mass ratio of methylamine hydrochloride to tin acetate is 0.634:1, the palladium-tin intermetallic compound is a palladium-tin intermetallic compound nanorod (Pd2Sn SNRs) with a length of 30 nm to 35 nm;

[0076] When the mass ratio of methylamine hydrochloride to tin acetate is 1.269:1, the palladium-tin intermetallic compound is a palladium-tin intermetallic compound nanorod (Pd2SnNRs) having a length of 70 nm to 75 nm;

[0077] When the mass ratio of methylamine hydrochloride to tin acetate is 2.537:1, the palladium-tin intermetallic compound is a palladium-tin intermetallic compound nanorod (Pd2Sn LNRs) having a length of 120 nm to 125 nm;

[0078] 2. Surface modification of palladium-tin intermetallic compounds:

[0079] The palladium-tin metal compound is dissolved in cyclohexane, and then a chloroform solution of soybean lecithin is added dropwise, and the solvent is evaporated in a rotary evaporator under vacuum at 60° C. to obtain the palladium-tin metal compound modified with soybean lecithin, namely, Pd2Sn-SPNDs, Pd2Sn-SP SNRs, Pd2Sn-SPNRs and Pd2Sn-SP LNRs;

[0080] The mass ratio of cyclohexane to the palladium-tin intermetallic compound is 790:1;

[0081] The mass ratio of soybean lecithin to palladium-tin intermetallic compound in the chloroform solution of soybean lecithin is 6.5:1;

[0082] The concentration of soybean lecithin in the chloroform solution of soybean lecithin is 1 mg / mL.

[0083] Figure 2 TEM images and elemental mapping images of Pd2Sn NDs and Pd2SnNRs prepared in step 1 of Example 1 at different magnifications; Figure 3 TEM images and elemental mapping images of Pd2Sn SNRs and Pd2Sn LNRs prepared in step 1 of Example 1 at different magnifications. Figure 2 and Figure 3It can be seen that methylamine hydrochloride plays an important role in controlling the morphology of palladium-tin intermetallic compounds. The figure includes transmission electron microscopy (TEM) images and element mapping diagrams of palladium-tin intermetallic compounds of different sizes. The palladium-tin intermetallic compounds show uniform and controllable morphology, as well as uniform distribution of corresponding elements, which confirms the successful construction of intermetallic compounds of different morphologies; the particle size of Pd2Sn NDs is 5nm~10nm; the length of Pd2Sn SNRs is 30nm~35nm; the length of Pd2Sn NRs is 70nm~75nm; the length of Pd2Sn LNRs is 120nm~125nm.

[0084] Figure 4 High-resolution transmission electron microscope images and lattice spacing measurements of Pd2Sn NRs and Pd2Sn NDs prepared in step 1 of Example 1. As can be seen from the figure, the interface lattice spacings displayed by Pd2Sn NRs and Pd2Sn NDs are 0.195nm and 0.236nm, respectively, which are orthorhombic phase (320) and (021) crystal planes.

[0085] Figure 5 This is the EDS measurement spectrum of Pd2Sn NRs prepared in step 1 of Example 1. As can be seen from the figure, the molar ratio of palladium and tin elements coexisting is 2:1, proving the successful preparation of palladium-tin intermetallic compound.

[0086] Figure 6 The PXRD images of Pd2Sn NDs, Pd2Sn SNRs, Pd2Sn NRs and Pd2Sn LNRs prepared in step 1 of Example 1 are shown in Figure 1. a is a Pd2Sn NRs and Pd2Sn NDs, b is a local enlarged view of a, and c is a Pd2Sn LNRs and Pd2Sn SNRs. As can be seen from the figure, their diffraction peaks all have good crystallinity, which can match the diffraction peaks of the pure orthorhombic Pd2Sn phase (PDF00-026-1297), and the lattice parameters are all It shows a cotunnite structure.

[0087] Figure 7 The XPS measurement spectra of Pd2SnNRs and Pd2SnNDs prepared in step 1 of Example 1. As can be seen from the figure, the prepared palladium-tin intermetallic compound is mainly composed of Pd and Sn elements.

[0088] Figure 8 The high-resolution XPS measurement spectra of the Pd 3d and Sn 3d energy levels of Pd2SnNRs and Pd2SnNDs prepared in step 1 of Example 1. As can be seen from the figure, the palladium 3d energy level can be a spin-split orbital 3d 3 / 2 and 3D 5 / 2, the binding energies at 341.4 eV and 336.1 eV are attributed to Pd 2+ , while the peaks at 340.6 eV and 335.3 eV are assigned to Pd0, which confirms that Pd 2+ (76%) and Pd0 (24%) coexist, while Pd 2+ (64%) and Pd0 (36%) coexist. At the same time, the high-resolution XPS spectrum of Sn 3d of the Pd2Sn intermetallic compound shows obvious decomposition, verifying the existence of tin with two different valence states, at 495.3eV (3d 5 / 2 ) and 486.8eV(3d 3 / 2 ) and Sn 4+ Correlation, and at 493.8eV (3d 5 / 2 ) and 485.3eV(3d 3 / 2 ) and Sn 2+ These results confirm that Pd2Sn intermetallic compounds can generate more reactive oxygen species (ROS) through redox reactions.

[0089] With 808nm laser (0.8W / cm 2 ) was continuously irradiated with a 200 μg / mL aqueous solution of Pd2Sn-SPNRs for 4 cycles to explore its photothermal stability, and the temperature changes during the hot and cold cycles were plotted ( Fig. 9 b) Select the cooling curve of the first cycle and calculate the photothermal conversion efficiency (η) of the Pd2Sn-SP aqueous solution ( Fig. 9 a). Fig. 9 The photothermal stability test diagram of Pd2Sn-SPNRs aqueous solution, a is the photothermal conversion efficiency, b is the change of hot and cold cycle temperature; Fig. 9 It can be seen that Pd2Sn-SPNRs have good photothermal conversion efficiency. In addition to the photothermal conversion ability, photothermal stability is also crucial to the photothermal conversion process and was further evaluated by four on / off laser power cycles. After 4 cycles of heating and natural cooling, there was no obvious change in temperature, which indicates that they have high photothermal stability ( Fig. 9 b). According to the cooling curve, the photothermal conversion efficiency (η) of Pd2Sn-SPNRs was calculated to be 41.2% ( Fig. 9 a).

[0090] The absorbance values ​​of the palladium-tin intermetallic compounds modified with soybean lecithin at different concentrations at 808 nm were statistically analyzed in the UV-vis-NIR absorption spectrum test ( Fig.12The corresponding absorbance value at 808 nm of each curve in the figure is plotted to draw a fitting curve of the mass extinction coefficient of the palladium-tin intermetallic compound modified with soybean lecithin, and the slope of the fitting curve is its extinction coefficient a; Fig.10 : The fitting curve of the mass extinction coefficient of the palladium-tin intermetallic compound modified with soybean lecithin prepared in Example 1, 1 is Pd2Sn-SPNRs, 2 is Pd2Sn-SPNDs; It can be seen from the figure that the absorbance of Pd2Sn-SPNDs and Pd2Sn-SPNRs increases linearly with the increase of concentration, and the extinction coefficient of Pd2Sn-SPNRs is a=5.33L g -1 cm -1 , the extinction coefficient of Pd2Sn-SPNDs is a=2.30L g - 1 cm -1 ; From the extinction coefficient, Pd2Sn-SPNRs (5.33L g -1 cm -1 ) than Pd2Sn-SPNDs (2.30L g -1 cm -1 ) has stronger absorption.

[0091] In order to make the Pd2Sn intermetallic compound have higher biocompatibility, the palladium-tin intermetallic compound modified with soybean lecithin was prepared. Fig.11 The zeta potential of Pd2Sn NRs prepared in step 1 of Example 1 and Pd2Sn-SPNRs prepared in step 2. As can be seen from the figure, after SP functionalization, the zeta potential changes from 0.13 mV to -29.93 mV.

[0092] The Pd2Sn-SPNRs and Pd2Sn-SPNDs prepared in Example 1 were dispersed in water and subjected to UV-vis-NIR absorption spectrum test. Fig.12 The UV-vis-NIR absorption spectra of Pd2Sn-SPNRs aqueous solution and Pd2Sn-SPNDs aqueous solution, 1 is a concentration of 400μg / mL, 2 is a concentration of 300μg / mL, 3 is a concentration of 200μg / mL, 4 is a concentration of 100μg / mL, 5 is a concentration of 50μg / mL, and 6 is a concentration of 25μg / mL. It can be seen from the figure that the absorbance intensity of Pd2Sn-SPNRs and Pd2Sn-SP NDs increases linearly with the increase of concentration.

[0093] The characterization of the ions was qualitatively evaluated by electron spin resonance (ESR) measurements using 2,2,6,6-tetramethylpiperidine (TEMP) and 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) as trapping agents. 1 The generation of O2 and ·OH. Using TEMP as a trapping agent, the detection of ·1 O2( Fig.13 a) The Pd2Sn-SPNRs aqueous solution prepared in Example 1 (100 μL, 1 mg / mL), PBS (340 μL, pH=5.5) and 2,2,6,6-tetramethylpiperidine (TEMP) (10 μL) were mixed. The hydrogen peroxide group was injected with hydrogen peroxide (100 mM, 50 μL) at high speed. The laser irradiation group was irradiated with 808 nm laser (0.8 W / cm 2 ) irradiation; DMPO was used as the trapping agent to detect ·OH( Fig.13 b) The Pd2Sn-SP NRs aqueous solution (100 μL, 1 mg / mL) prepared in Example 1, PBS (340 μL, pH=5.5) and 5,5-dimethyl-1-pyrrolidinyl-N-oxide (DMPO) (10 μL) were mixed, and hydrogen peroxide (100 mM, 50 μL) was quickly injected. The solution was analyzed by electron paramagnetic resonance spectrometer. The laser irradiation group used 808 nm laser (0.8 W / cm 2 ) irradiation. Fig.13 This is the ESR image of Pd2Sn-SPNRs prepared in Example 1, a is the detection 1 O2, b is to detect OH. Fig.13 It can be seen that when Pd2Sn-SPNRs are irradiated with 808nm laser, 1 The signal peak of O2 is obviously 1:1:1, and the signal is stronger after adding hydrogen peroxide, indicating that 1 O2. Fig.13 In b, an obvious quadruple resonance peak of ·OH with a signal intensity ratio of 1:2:2:1 can be observed, verifying the generation of ·OH. At the same time, under 808nm laser irradiation, the quadruple resonance peak signal will be enhanced.

[0094] 3 mL of phosphate buffer solution (pH = 5.5) containing 300 μg / mL TMB (or OPD) and 100 μg / mL Pd2Sn-SPNRs was mixed with hydrogen peroxide to make the concentration of hydrogen peroxide in the solution 50 mM. After a certain reaction time, the absorbance intensity of each group was recorded. The laser irradiation group used 808 nm laser (0.8 W / cm 2 ) irradiation, and the control group did not add hydrogen peroxide and did not use laser irradiation. Fig.14This is the UV-visible absorption spectrum of the Pd2Sn-SPNRs prepared in Example 1 for catalytic oxidation of OPD and TMB under different conditions. a is OPD, b is TMB, 1 is Pd2Sn-SPNRs+hydrogen peroxide+laser irradiation, 2 is Pd2Sn-SPNRs+hydrogen peroxide, 3 is the laser irradiation group alone, and 4 is the control group. As can be seen from the figure, after the addition of hydrogen peroxide, Pd2Sn-SPNRs induced the production of significant characteristic absorption of the oxidation products oxOPD (420nm) or oxTMB (652nm). There was no change in both the control group and the laser group alone. In addition, after laser irradiation, the absorption intensity of Pd2Sn-SP was enhanced, which is consistent with the above results. Fig.13 The ESR measurements showed similar results.

[0095] The simulated peroxidase activity of Pd2Sn-SP nanocomposites (NDs, NRs, SNRs and LNRs) modified with soybean lecithin of different morphologies was determined: TMB was used as substrate in phosphate buffer solution (PBS, pH = 5.5) in the presence of H2O2, and steady-state kinetic experiments were performed in phosphate buffer solution (pH = 5.5) in the presence of H2O2 and TMB with Pd2Sn-SP nanocomposites aqueous solution (20 μg / mL) as catalyst. At the same time, kinetic detection of Pd2Sn-SP nanocomposites was carried out with H2O2 as substrate (1, 2, 4 and 16 mM). All reactions were monitored by measuring the absorbance after different reaction times, and the Michaelis constant and maximum reaction rate were calculated by the formula according to the Michaelis-Menten equation.

[0096] Fig.15 The Michaelis-Menten kinetic analysis images and Lineweaver-Burk peroxidase simulation activity images of Pd2Sn-SP LNRs, Pd2Sn-SPNRs, Pd2Sn-SP SNRs and Pd2Sn-SPNDs prepared in Example 1, a is the Michaelis-Menten diagram, b is the Lineweaver-Burk diagram, 1 is Pd2Sn-SP LNRs, 2 is Pd2Sn-SPNRs, 3 is Pd2Sn-SP SNRs, and 4 is Pd2Sn-SPNDs. Table 1 is a comparison of the kinetic parameters of the peroxidase activity of palladium-tin intermetallic compounds of different morphologies prepared in Example 1. Fig.15 Table 1 shows the differences in catalytic activity of soybean lecithin-modified Pd2Sn-SP nanocomposites (NDs, NRs, SNRs and LNRs) with different morphologies through steady-state kinetic analysis, all of which are consistent with the typical Michaelis-Menten kinetics. According to the Lineweaver-Burk plot, the maximum reaction rate (V max) and Michaelis-Menten constant (Km), and are summarized in Table 1. In general, V max The higher the K m The lower the V, the better the catalytic performance. max and K m In terms of catalytic performance, Pd2Sn-SPNRs have higher catalytic efficiency than Pd2Sn-SPNDs. In addition, the catalytic efficiency is also related to the length of Pd2Sn-SP NRs. If it is too long or too short, it is not conducive to the POD simulation activity.

[0097] Table 1

[0098] Nanozymes <![CDATA[Pd2Sn-SPLNRs]]> <![CDATA[Pd2Sn-SPNRs]]> <![CDATA[Pd2Sn-SPSNRs]]> <![CDATA[Pd2Sn-SPNDs]]> Substrate <![CDATA[H2O2]]> <![CDATA[H2O2]]> <![CDATA[H2O2]]> <![CDATA[H2O2]]> <![CDATA[V max (×10 -8 Ms -1 )]]> 25.28 29.35 16.63 6.69 <![CDATA[K max (mM)]]> 22.65 20.86 23.61 17.27

[0099] 3 mL of phosphate buffer solution containing 300 μg / mL TMB and 100 μg / mL Pd2Sn-SPNRs was reacted at room temperature for a certain period of time, and the absorbance intensity of each group was recorded. Fig.16 The oxidase-like enzyme-like activity of Pd2Sn-SPNRs prepared in Example 1 at different times, 1 is 10min, 2 is 8min, 3 is 6min, 4 is 4min, and 5 is 2min. This figure shows the OXD-simulated catalytic activity of Pd2Sn-SPNRs (70nm-75nm) verified by TMB, producing O2; and the absorbance intensity at 652nm increases with time, indicating that Pd2Sn-SPNRs has obvious OXD-simulated activity and has oxidation ability in the absence of hydrogen peroxide.

[0100] A 3 mL aqueous solution containing 10 μg / mL MB and 100 μg / mL Pd2Sn-SPNRs was quickly injected with hydrogen peroxide solution to make the hydrogen peroxide concentration in the solution reach 50 μM. The absorbance of the mixed solution was detected at different time intervals, and MB was used to verify the POD simulation catalytic activity of Pd2Sn-SPNRs. Fig.17 The degradation images of methylene blue (MB) catalyzed by Pd2Sn-SPNRs prepared in Example 1 at different time points are shown in Figure 1, 0 min, 2 min, 3 min, 4 min, 6 min, 5 min, and 6 min. The methylene blue (MB) experiment verified the effective generation of ·OH in the presence of Pd2Sn-SPNRs, indicating that Pd2Sn-SPNRs have high POD simulation catalytic activity.

[0101] Fig.18 and Fig.19The invention relates to the catalase-like activity of Pd2Sn-SP LNRs, Pd2Sn-SPNRs, Pd2Sn-SP SNRs and Pd2Sn-SPNDs9 prepared in Example 1 under different conditions and different morphologies. The experiment uses a dissolved oxygen meter to detect the O2 generation induced by Pd2Sn-SP under different conditions and different morphologies to evaluate the CAT simulation activity: 3 mL Pd2Sn-SP LNRs, Pd2Sn-SPNRs, Pd2Sn-SP SNRs or Pd2Sn-SPNDs aqueous solutions (0, 50, 100, 200 and 400 μg / mL) are mixed with hydrogen peroxide so that the concentration of hydrogen peroxide in the solution is 50 mM, and finally the oxygen concentration (mg / L) is continuously recorded for 6 minutes. Fig.18 The Pd2Sn-SPNRs prepared in Example 1 were illuminated at different concentrations and 808 nm laser (0.8 W / cm 2 ) Catalase-like activity under irradiation conditions, a is the catalase activity of Pd2Sn-SPNRs at different concentrations, 1 is 400μg / mL, 2 is 200μg / mL, 3 is 100μg / mL, 4 is 50μg / mL, 5 is pure water, b is the effect of laser irradiation on the catalase-like activity of Pd2Sn-SPNRs, 1 is 200μg / mL, 2 is 200μg / mL+808nm laser irradiation; Fig.19 The palladium-tin intermetallic compounds of different morphologies prepared in Example 1 produce catalase-like activity under laser irradiation, 1 is 400μg / mL, 2 is 200μg / mL, 3 is 100μg / mL, 4 is 50μg / mL, and 5 is pure water; by comparison, it can be found that Pd2Sn-SP NRs exhibit the strongest CAT simulated catalytic activity, which is consistent with the results of POD simulated catalytic activity. As the concentration of Pd2Sn-SP NRs increases, the generation of O2 also increases, and the addition of laser further promotes the CAT simulated catalytic activity.

[0102] Fig. 20 The effect of the Pd2Sn-SP NRs prepared in Example 1 on cell activity when incubated with normal cells (L929 cells) at different concentrations for 12 h and 24 h; as can be seen from the figure, the Pd2Sn-SP NRs prepared in Example 1 have almost no cytotoxicity after incubation with L929 cells for 12 h and 24 h, and show good biocompatibility even at higher concentrations.

Claims

1. A method for preparing a morphology-controllable palladium-tin intermetallic compound, Features It is carried out in the following steps:

1. Preparation of palladium-tin intermetallic compounds by high temperature pyrolysis: Under magnetic stirring conditions, oleylamine, methylamine hydrochloride, acetylacetonate palladium and tin acetate are uniformly mixed to obtain a mixed solution A; under a vacuum state, the mixed solution A is heated to 40°C to 45°C, and kept warm for 20min to 25min at a temperature of 40°C to 45°C, the vacuum device is closed, nitrogen is introduced, and the temperature is kept at 55°C to 60°C for 30min to 35min to form a uniform solution, trioctylphosphine is added to the uniform solution, and the temperature is kept at 200°C to 210°C for 30min to 35min to obtain a mixed solution B, the mixed solution B is heated to 300°C to 310°C, and the temperature is 300°C to 310°C for 25min to 30min, and after the reaction is completed, the mixed solution is naturally cooled to room temperature, and the solution is collected by centrifugation and washed to obtain a palladium-tin intermetallic compound; When the mass ratio of methylamine hydrochloride to tin acetate is (0-0.25):1, the palladium-tin intermetallic compound is a nanodot with a particle size of 5nm-10nm; When the mass ratio of methylamine hydrochloride to tin acetate is (0.5-0.75):1, the palladium-tin intermetallic compound is a nanorod with a length of 30 nm to 35 nm; When the mass ratio of methylamine hydrochloride to tin acetate is (1.25-1.5):1, the palladium-tin intermetallic compound is a nanorod with a length of 70 nm to 75 nm; When the mass ratio of methylamine hydrochloride to tin acetate is (2.5-2.75):1, the palladium-tin intermetallic compound is a nanorod with a length of 120 nm to 125 nm; 2. Surface modification of palladium-tin intermetallic compounds: The palladium-tin metal compound is dissolved in cyclohexane, and then a chloroform solution of soybean lecithin is added dropwise, and the solvent is evaporated in a rotary evaporator under vacuum at a temperature of 60° C. to obtain the palladium-tin metal compound modified with soybean lecithin.

2. A method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features The mass ratio of oleylamine to tin acetate in step one is (0.30-0.35):1; the mass ratio of palladium acetylacetonate to tin acetate in step one is (1.70-1.75):

1.

3. A method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features The mass ratio of trioctylphosphine to tin acetate described in step 1 is (0.30-0.35):

1.

4. A method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features In step 1, oleylamine, methylamine hydrochloride, palladium acetylacetonate and tin acetate are mixed at a rotation speed of 500 rpm to 600 rpm for 5 min to 10 min to obtain a mixed solution A.

5. A method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features In step 1, the mixed solution A is heated to 40°C to 45°C at a heating rate of 2°C / min to 3°C / min.

6. A method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features In step 1, the mixed solution B is heated to 300° C. to 310° C. at a heating rate of 2° C. / min to 3° C. / min.

7. A method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features The washing described in step 1 is washing with ethanol and chloroform alternately.

8. The method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features The mass ratio of cyclohexane to the palladium-tin intermetallic compound described in step 2 is (790-795):

1.

9. The method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features The mass ratio of soybean lecithin to palladium-tin intermetallic compound in the chloroform solution of soybean lecithin described in step 2 is (6.0-6.5):

1.

10. The method for preparing a morphology-controllable palladium-tin intermetallic compound according to claim 1, Features The concentration of soybean lecithin in the chloroform solution of soybean lecithin described in step 2 is 1 mg / mL to 1.5 mg / mL.

Citation Information

Patent Citations

  • Catalase-entrapped liposome connected with PD-L1 antibody and preparation method thereof

    CN110898012A

  • Apolipoprotein modified fusion type multifunctional nano vesicle, and preparation method and application thereof

    CN113616811A

  • Preparation method and application of two-dimensional flaky manganite nano-enzyme

    CN116621227A

  • Potential of hydrogen (pH) controlled release polymetallic nano-enzyme as well as preparation method and application of polymetallic nano-enzyme

    CN117503926A