Ni and Co bimetallic alloy-strontium titanate composite photocatalyst as well as preparation method and application thereof
Through the preparation of Ni,Co bimetal alloy-strontium titanate composite photocatalyst, the problem of strontium titanate relying on precious metal cocatalysts in the prior art is solved, and economical and efficient photocatalytic decomposition of water to prepare hydrogen, with excellent light Catalytic performance and stability.
Patent Information
- Application Number
- CN202410967741.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-18
AI Technical Summary
In the prior art, strontium titanate, as a photocatalyst, relies on precious metal cocatalysts when decomposing water to prepare hydrogen, resulting in high cost and low efficiency problems, and lack of an economical, efficient and stable non-precious metal cocatalyst system.
Ni is prepared by mixing Al-doped strontium titanate with a metal-organic frame containing Ni,Co bimetallic bimetallic and reducing reaction under an ammonia atmosphere. Co bimetallic alloy-strontium titanate composite photocatalyst was prepared by hydrothermal method and molten salt treatment method, and the NiCo alloy cocatalyst was supported on the surface of strontium titanate.
Achieve economical and efficient photocatalytic complete decomposition of hydrogen production in aquatic products. The photocatalytic hydrogen production rate reaches 979.9μmolg-1h-1, the quantum efficiency is 11.9%, and it has good photocatalytic hydrogen production stability, which overcomes the high cost of precious metals. question.
Smart Images

Figure CN118904346A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogen energy preparation, relates to a photocatalytic clean preparation technology of hydrogen energy, and specifically relates to a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst and a preparation method and application thereof. Background Art
[0002] The development of society depends to a large extent on the development and utilization of energy. With the continuous advancement of industrialization, the environmental pollution and energy shortage caused by the massive consumption of fossil energy have gradually attracted people's attention. Therefore, the development of clean and efficient renewable energy is of great significance to the sustainable development of human society. H2 has the characteristics of high energy density, easy storage and transportation, and no carbon emissions, making it the most ideal secondary energy source. Using abundant solar energy to drive the preparation of H2 is a technology with great development potential. Using solar energy to drive photocatalysts to decompose water to produce hydrogen is one of the most ideal and simplest ways to convert solar energy into hydrogen energy. The key to this technology lies in the development and utilization of economical, efficient and stable photocatalyst systems.
[0003] The principle of photocatalytic complete decomposition of water to produce hydrogen is: under the irradiation of light of a certain energy, the semiconductor photocatalyst is excited by light to produce electron-hole pairs, and then the electrons migrate to the catalyst surface to reduce water to hydrogen, while the holes migrate to the catalyst surface to oxidize water to oxygen. According to existing research, strontium titanate is a photocatalyst with great potential, but its excellent photocatalytic performance depends on precious metal co-catalysts, which will seriously restrict the application of solar photocatalytic decomposition of water to produce hydrogen. Therefore, it is of great significance to develop an economical, efficient and stable non-precious metal co-catalyst system. Summary of the invention
[0004] The purpose of the present invention is to provide a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst and a preparation method and application thereof, so as to realize economical and efficient photocatalytic hydrogen production by the photocatalyst.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst comprises the following steps:
[0007] After Al-doped strontium titanate and a metal-organic framework containing Ni, Co bimetallics are uniformly mixed, a reduction reaction is carried out in an ammonia atmosphere to obtain a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst.
[0008] Furthermore, Al-doped strontium titanate is prepared by a hydrothermal method and molten salt.
[0009] Furthermore, the molar ratio of Ni to Co in the metal-organic framework containing Ni, Co bimetallic is 1:0.1-1.
[0010] Furthermore, the mass ratio of Al-doped strontium titanate to the metal-organic framework containing Ni, Co bimetallic is 100 mg: 1-10 mg.
[0011] Furthermore, the uniform mixing is carried out by grinding or dispersing the Al-doped strontium titanate and the metal-organic framework containing Ni, Co bimetallic in a solvent and then evaporating to dryness.
[0012] Furthermore, the ammonia flow rate is 20-100 mL / min.
[0013] Furthermore, the reduction reaction temperature is 600-1000° C., and the time is 1-5 h.
[0014] Further, the temperature is increased to 600-1000° C. at a heating rate of 5-10° C. / min.
[0015] A Ni, Co bimetallic alloy-strontium titanate composite photocatalyst prepared according to the method.
[0016] The invention discloses an application of a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst prepared according to the method in photocatalytic hydrogen production.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The catalyst preparation method of the present invention uses a metal-organic framework (NiCo-MOF) containing Ni and Co bimetallics as a precursor to prepare a NiCo alloy co-catalyst for the first time, and loads the NiCo bimetallic alloy as a co-catalyst on the surface of Al-doped strontium titanate, thereby achieving the generation and loading of the alloy co-catalyst in one step. The raw materials are cheap and easy to obtain, and the preparation scheme is simple and easy to repeat, which overcomes the problem of using precious metals and high costs in the prior art. The Ni, Co bimetallic alloy-strontium titanate composite photocatalyst prepared by the present invention has excellent photocatalytic performance of completely decomposing water to produce hydrogen and oxygen. The photocatalytic hydrogen production rate reaches 979.9μmolg -1 h -1 The quantum efficiency at 350nm is 11.9%, and it has good stability in photocatalytic hydrogen production. The invention is simple to operate and has good repeatability, and provides a reliable solution for the development and application of economical, efficient and stable new photocatalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 are X-ray diffraction (XRD) patterns of NiCo bimetallic alloy (MOF-NH3), Al-doped strontium titanate (STO), and Al-doped strontium titanate loaded with NiCo bimetallic alloy (3%-MOF-STO-NH3);
[0020] Figure 2 These are scanning electron microscope (SEM) and transmission electron microscope (TEM) images of 3%-MOF-STO-NH3 of Example 2; wherein a) is SEM and b) is TEM;
[0021] Figure 3 is the photocatalytic hydrogen production rate diagram of Al-doped strontium titanate loaded with different proportions of NiCo bimetallic alloy;
[0022] Figure 4 This is a photocatalytic hydrogen production stability test diagram of 3%-MOF-STO-NH3 in Example 2. DETAILED DESCRIPTION
[0023] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0024] The present invention utilizes solar energy to realize the technology of cheaply producing hydrogen energy by photocatalytic decomposition of water. Specifically, a reliable preparation scheme of a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst is utilized to realize the photocatalytic complete decomposition of water to produce hydrogen and oxygen, which is beneficial to the industrial application of photocatalytic decomposition of water to produce hydrogen.
[0025] The preparation method of a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst of the present invention is as follows: cobalt nitrate, nickel nitrate, polyvinyl pyrrolidone and trimesic acid are dispersed in a mixed solution of H2O, ethanol and N,N-dimethylformamide, and the product is washed and centrifugally dried after a hydrothermal reaction to obtain a metal-organic framework (NiCo-MOF) containing Ni, Co bimetallic. Then, Al-doped strontium titanate is prepared by a conventional hydrothermal method and a molten salt treatment method. Specifically, the above-mentioned metal-organic framework and strontium titanate are dispersed in an ethanol solution, and stirred and evaporated in an oil bath. Subsequently, the obtained sample is calcined in an ammonia atmosphere to obtain a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst.
[0026] Specifically, the preparation method comprises the following steps:
[0027] Step 1: Add 10mmol of titanic acid butyric acid and 20mL of ethylene glycol to the hydrothermal kettle. Add 20mL of water to a beaker and add 10mmol of strontium nitrate, and dissolve it by ultrasonic. Drop the solution in the beaker into the hydrothermal kettle, pour it all in after the gel is formed, and turn the agitator to the maximum. Then add 10mL of sodium hydroxide solution (5mol / L) to the hydrothermal kettle and stir at 1000rpm for 30min. After stirring, tighten the hydrothermal kettle, place it in an oven, heat it at 200℃ for 24h, and place it in a ventilated place to cool naturally to room temperature after heating. After taking it out, wash the sample with deionized water to pH~7. Put the washed sample into a blast drying oven and dry it at 60℃ for 12h.
[0028] Step 2: Mix the strontium titanate, SrCl2, and Al2O3 obtained in step 1 in a molar ratio of 1:10:0.02 and grind them in a mortar. Place the mixed material in a crucible, heat it to 1100°C in a muffle furnace at a heating rate of 5°C per minute, hold for 5 hours, and then cool it naturally to room temperature. Ultrasonic dissolve the sample taken out in 50mL deionized water, centrifuge and wash it 5 times, and place the washed sample in a drying oven at 60°C for 12 hours. The Al-doped SrTiO3 after molten salt treatment is named STO.
[0029] Step 3: Prepare a mixed solution with a volume ratio of H2O: N, N-dimethylformamide: ethanol of 1-2: 1-3: 1-2. Dissolve 0.216g of nickel salt (Ni(NO3)2·6H2O, nickel chloride or nickel sulfate), 0.216g of cobalt salt (Co(NO3)2·6H2O, cobalt chloride or cobalt sulfate), trimesic acid, and polyvinyl pyrrolidone (molecular weight of 8000-700000) in the above mixed solution. When the mass of nickel salt is 0.216g, the volume of the mixed solution is 30mL. Ultrasonicate at room temperature for 30min, and then transfer the solution to a 50mL polytetrafluoroethylene hydrothermal autoclave. Place the hydrothermal autoclave in an oven, heat at 150℃ for 10h, and cool naturally to room temperature. Wash the prepared sample, centrifuge and dry it to obtain a metal-organic framework containing Ni, Co bimetallics, and name the sample NiCo-MOF. The molar ratio of the nickel salt to the cobalt salt is 1:0.1-1, the mass ratio of trimesic acid to polyvinyl pyrrolidone is 1:1-12. The molar ratio of the nickel salt to trimesic acid is 1:1.
[0030] In the present invention, the nickel salt is described by taking Ni(NO3)2·6H2O as an example, and nickel chloride or nickel sulfate may also be used.
[0031] In the present invention, the cobalt salt is described by taking Co(NO3)2·6H2O as an example, and cobalt chloride or cobalt sulfate may also be used.
[0032] Step 4: Disperse 100 mg STO and 1-10 mg NiCo-MOF in 5-10 mL ethanol (water or methanol) to obtain a suspension. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and set the oil bath temperature to 80 ° C. Alternatively, fully grind and mix 100 mg STO and 1-10 mg NiCo-MOF. Place the above samples in a tubular furnace filled with ammonia for high-temperature reduction. The specific experimental parameters are: NH3 flow rate of 20-100 mL / min, heating rate of 5-10 ° C / min, heating temperature of 600-1000 ° C, and heating time of 1-5h.
[0033] Step 5: Add the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst prepared in step 4 into pure water to conduct a photocatalytic water decomposition hydrogen production test. The specific steps are as follows:
[0034] 1) Add 10 mg of Ni, Co bimetallic alloy-strontium titanate composite photocatalyst to a reactor with a volume of 105 mL, and add deionized water with a total volume of 80 mL;
[0035] 2) Before irradiation, argon gas was purged into the reactor for 15 min to remove oxygen from the system;
[0036] 3) Turn on the magnetic stirrer and the xenon lamp.
[0037] The present invention uses a metal-organic framework (NiCo-MOF) containing Ni and Co bimetallics as a precursor, loads a NiCo alloy co-catalyst on the surface of Al-doped strontium titanate, realizes the preparation of a bimetallic alloy, and loads the bimetallic alloy as a co-catalyst on the surface of strontium titanate. The prepared NiCo alloy-loaded strontium titanate can completely decompose water and exhibits good photocatalytic hydrogen production activity. The photocatalytic hydrogen production rate reaches 979.9 μmol g -1 h -1 The quantum efficiency at 350nm is 11.9%, and it has good stability in photocatalytic hydrogen production. The invention is simple to operate and has good repeatability, and provides a reliable solution for the development and application of economical, efficient and stable new photocatalysts.
[0038] The following are specific embodiments.
[0039] Comparative Example 1
[0040] Step 1: Add 10mmol of titanic acid butyric acid and 20mL of ethylene glycol to the hydrothermal kettle. Add 20mL of water and 10mmol of strontium nitrate to a beaker and dissolve by ultrasonication. Drop the solution in the beaker into the hydrothermal kettle, pour it all in after the gel is formed, and turn the agitator to the maximum. Then add 10mL of sodium hydroxide solution (5mol / L) to the hydrothermal kettle and stir at 1000rpm for 30min. After stirring, tighten the hydrothermal kettle, place it in an oven, heat it at 200℃ for 24h, and place it in a ventilated place to cool naturally to room temperature after heating. After taking it out, wash the sample with deionized water to pH~7. Place the washed sample in a blast drying oven and dry it at 60℃ for 12h to obtain strontium titanate.
[0041] Step 2: Mix the strontium titanate, SrCl2, and Al2O3 obtained in step 1 in a molar ratio of 1:10:0.02 and grind them in a mortar. Place the mixed material in a crucible, heat it to 1100°C in a muffle furnace at a heating rate of 5°C per minute, maintain for 5 hours, and then cool it naturally to room temperature. Ultrasonic dissolve the sample taken out in 50mL deionized water, centrifuge and wash it 5 times, put the washed sample into a drying oven and dry it at 60°C for 12 hours to obtain Al-doped SrTiO3. The Al-doped SrTiO3 after molten salt treatment is named STO.
[0042] Step 3: Add the STO prepared in step 2 into pure water for photocatalytic water decomposition and hydrogen production test. The specific steps are as follows:
[0043] 1) Add 10 mg of STO photocatalyst to a reactor with a volume of 105 mL and add deionized water with a total volume of 80 mL;
[0044] 2) Before irradiation, argon gas was purged into the reactor for 15 min to remove oxygen from the system;
[0045] 3) Turn on the magnetic stirrer and the xenon lamp.
[0046] Comparative Example 2
[0047] Step 1: Prepare a solution with a volume ratio of H2O: N, N-dimethylformamide: ethanol of 1:1:1. Dissolve 0.216g Ni(NO3)2·6H2O, 0.216g Co(NO3)2·6H2O, 0.15g trimesic acid, and 1.5g polyvinyl pyrrolidone in 30mL of the above solution. Ultrasonicate at room temperature for 30min, and then transfer the solution to a 50mL polytetrafluoroethylene hydrothermal autoclave. Place the hydrothermal autoclave in an oven, heat at 150℃ for 10h, and cool naturally to room temperature. Wash the prepared sample, centrifuge and dry it, and name the sample NiCo-MOF.
[0048] Step 2: Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction. The specific experimental parameters are: NH3 flow rate of 28mL / min, heating rate of 5℃ / min, heating temperature of 800℃, and heating time of 2h. The prepared sample is named MOF-NH3.
[0049] Example 1
[0050] Step 1: Add 10mmol of titanic acid butyric acid and 20mL of ethylene glycol to the hydrothermal kettle. Add 20mL of water to a beaker and add 10mmol of strontium nitrate, and dissolve it by ultrasonic. Drop the solution in the beaker into the hydrothermal kettle, pour it all in after the gel is formed, and turn the agitator to the maximum. Then add 10mL of sodium hydroxide solution (5mol / L) to the hydrothermal kettle and stir at 1000rpm for 30min. After stirring, tighten the hydrothermal kettle, place it in an oven, heat it at 200℃ for 24h, and place it in a ventilated place to cool naturally to room temperature after heating. After taking it out, wash the sample with deionized water to pH~7. Put the washed sample into a blast drying oven and dry it at 60℃ for 12h.
[0051] Step 2: Mix the strontium titanate, SrCl2, and Al2O3 obtained in step 1 in a molar ratio of 1:10:0.02 and grind them in a mortar. Place the mixed material in a crucible, heat it to 1100°C in a muffle furnace at a heating rate of 5°C per minute, hold for 5 hours, and then cool it naturally to room temperature. Ultrasonic dissolve the sample taken out in 50mL deionized water, centrifuge and wash it 5 times, and place the washed sample in a drying oven at 60°C for 12 hours. The Al-doped SrTiO3 after molten salt treatment is named STO.
[0052] Step 3: Prepare a solution with a volume ratio of H2O: N, N-dimethylformamide: ethanol of 1:1:1. Dissolve 0.216g Ni(NO3)2·6H2O, 0.216g Co(NO3)2·6H2O, 0.15g trimesic acid, and 1.5g polyvinyl pyrrolidone in 30mL of the above solution. Ultrasonicate at room temperature for 30min, and then transfer the solution to a 50mL polytetrafluoroethylene hydrothermal autoclave. Place the hydrothermal autoclave in an oven, heat at 150℃ for 10h, and cool naturally to room temperature. Wash the prepared sample, centrifuge and dry it, and name the sample NiCo-MOF.
[0053] Step 4: Disperse 100 mg of STO and 1 mg of NiCo-MOF in 5 mL of ethanol. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and the oil bath temperature is set to 80°C. Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction. The specific experimental parameters are: NH3 flow rate of 28 mL / min, heating rate of 5°C / min, heating temperature of 800°C, and heating time of 2h. The prepared sample is named 1%-MOF-STO-NH3.
[0054] Step 5: Add the 1%-MOF-STO-NH3 prepared in step 4 into pure water for photocatalytic water decomposition and hydrogen production test. The specific steps are as follows:
[0055] 1) Add 10 mg of Al-doped strontium titanate photocatalyst loaded with NiCo alloy into a reactor with a volume of 105 mL, and add deionized water with a total volume of 80 mL;
[0056] 2) Before irradiation, argon gas was purged into the reactor for 15 min to remove oxygen from the system;
[0057] 3) Turn on the magnetic stirrer and the xenon lamp.
[0058] Example 2
[0059] Step 1: Add 10mmol of titanic acid butyric acid and 20mL of ethylene glycol to the hydrothermal kettle. Add 20mL of water to a beaker and add 10mmol of strontium nitrate, and dissolve by ultrasound. Drop the solution in the beaker into the hydrothermal kettle, pour it all in after the gel is formed, and turn the agitator to the maximum. Then add 10mL of sodium hydroxide solution (5mol / L) to the hydrothermal kettle and stir at 1000rpm for 30min. After stirring, tighten the hydrothermal kettle, place it in an oven, heat it at 200℃ for 24h, and place it in a ventilated place to cool naturally to room temperature after heating. After taking it out, wash the sample with deionized water to pH~7. Put the washed sample into a blast drying oven and dry it at 60℃ for 12h.
[0060] Step 2: Mix the strontium titanate, SrCl2, and Al2O3 obtained in step 1 in a molar ratio of 1:10:0.02 and grind them in a mortar. Place the mixed material in a crucible, heat it to 1100°C in a muffle furnace at a heating rate of 5°C per minute, hold for 5 hours, and then cool it naturally to room temperature. Ultrasonic dissolve the sample taken out in 50mL deionized water, centrifuge and wash it 5 times, and place the washed sample in a drying oven at 60°C for 12 hours. The Al-doped SrTiO3 after molten salt treatment is named STO.
[0061] Step 3: Prepare a solution with a volume ratio of H2O: N, N-dimethylformamide: ethanol of 1:1:1. Dissolve 0.216g Ni(NO3)2·6H2O, 0.216g Co(NO3)2·6H2O, 0.15g trimesic acid, and 1.5g polyvinyl pyrrolidone in 30mL of the above solution. Ultrasonicate at room temperature for 30min, and then transfer the solution to a 50mL polytetrafluoroethylene hydrothermal autoclave. Place the hydrothermal autoclave in an oven, heat at 150℃ for 10h, and cool naturally to room temperature. Wash the prepared sample, centrifuge and dry it, and name the sample NiCo-MOF.
[0062] Step 4: Disperse 100 mg of STO and 3 mg of NiCo-MOF in 5 mL of ethanol. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and the temperature of the oil bath is set to 80°C. Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction. The specific experimental parameters are: NH3 flow rate of 28 mL / min, heating rate of 5°C / min, heating temperature of 800°C, and heating time of 2h. The prepared sample is named 3%-MOF-STO-NH3.
[0063] Step 5: Add the 3%-MOF-STO-NH3 prepared in step 4 into pure water for photocatalytic water decomposition and hydrogen production test. The specific steps are as follows:
[0064] 1) Add 10 mg of Al-doped strontium titanate photocatalyst loaded with NiCo alloy into a reactor with a volume of 105 mL, and add deionized water with a total volume of 80 mL;
[0065] 2) Before irradiation, argon gas was purged into the reactor for 15 min to remove oxygen from the system;
[0066] 3) Turn on the magnetic stirrer and the xenon lamp.
[0067] Example 3
[0068] Step 1: Add 10mmol of titanic acid butyric acid and 20mL of ethylene glycol to the hydrothermal kettle. Add 20mL of water to a beaker and add 10mmol of strontium nitrate, and dissolve by ultrasound. Drop the solution in the beaker into the hydrothermal kettle, pour it all in after the gel is formed, and turn the agitator to the maximum. Then add 10mL of sodium hydroxide solution (5mol / L) to the hydrothermal kettle and stir at 1000rpm for 30min. After stirring, tighten the hydrothermal kettle, place it in an oven, heat it at 200℃ for 24h, and place it in a ventilated place to cool naturally to room temperature after heating. After taking it out, wash the sample with deionized water to pH~7. Put the washed sample into a blast drying oven and dry it at 60℃ for 12h.
[0069] Step 2: Mix the strontium titanate, SrCl2, and Al2O3 obtained in step 1 in a molar ratio of 1:10:0.02 and grind them in a mortar. Place the mixed material in a crucible, heat it to 1100°C in a muffle furnace at a heating rate of 5°C per minute, hold for 5 hours, and then cool it naturally to room temperature. Ultrasonic dissolve the sample taken out in 50mL deionized water, centrifuge and wash it 5 times, and place the washed sample in a drying oven at 60°C for 12 hours. The Al-doped SrTiO3 after molten salt treatment is named STO.
[0070] Step 3: Prepare a solution with a volume ratio of H2O: N, N-dimethylformamide: ethanol of 1:1:1. Dissolve 0.216g Ni(NO3)2·6H2O, 0.216g Co(NO3)2·6H2O, 0.15g trimesic acid, and 1.5g polyvinyl pyrrolidone in 30mL of the above solution. Ultrasonicate at room temperature for 30min, and then transfer the solution to a 50mL polytetrafluoroethylene hydrothermal autoclave. Place the hydrothermal autoclave in an oven, heat at 150℃ for 10h, and cool naturally to room temperature. Wash the prepared sample, centrifuge and dry it, and name the sample NiCo-MOF.
[0071] Step 4: Disperse 100 mg of STO and 5 mg of NiCo-MOF in 5 mL of ethanol. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and the oil bath temperature is set to 80°C. Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction. The specific experimental parameters are: NH3 flow rate of 28 mL / min, heating rate of 5°C / min, heating temperature of 800°C, and heating time of 2h. The prepared sample is named 5%-MOF-STO-NH3.
[0072] Step 5: Add the 5%-MOF-STO-NH3 prepared in step 4 into pure water for photocatalytic water decomposition and hydrogen production test. The specific steps are as follows:
[0073] 1) Add 10 mg of Al-doped strontium titanate photocatalyst loaded with NiCo alloy into a reactor with a volume of 105 mL, and add deionized water with a total volume of 80 mL;
[0074] 2) Before irradiation, argon gas was purged into the reactor for 15 min to remove oxygen from the system;
[0075] 3) Turn on the magnetic stirrer and the xenon lamp.
[0076] Example 4
[0077] Step 1: Add 10mmol of titanic acid butyric acid and 20mL of ethylene glycol to the hydrothermal kettle. Add 20mL of water to a beaker and add 10mmol of strontium nitrate, and dissolve by ultrasound. Drop the solution in the beaker into the hydrothermal kettle, pour it all in after the gel is formed, and turn the agitator to the maximum. Then add 10mL of sodium hydroxide solution (5mol / L) to the hydrothermal kettle and stir at 1000rpm for 30min. After stirring, tighten the hydrothermal kettle, place it in an oven, heat it at 200℃ for 24h, and place it in a ventilated place to cool naturally to room temperature after heating. After taking it out, wash the sample with deionized water to pH~7. Put the washed sample into a blast drying oven and dry it at 60℃ for 12h.
[0078] Step 2: Mix the strontium titanate, SrCl2, and Al2O3 obtained in step 1 in a molar ratio of 1:10:0.02 and grind them in a mortar. Place the mixed material in a crucible, heat it to 1100°C in a muffle furnace at a heating rate of 5°C per minute, hold for 5 hours, and then cool it naturally to room temperature. Ultrasonic dissolve the sample taken out in 50mL deionized water, centrifuge and wash it 5 times, and place the washed sample in a drying oven at 60°C for 12 hours. The Al-doped SrTiO3 after molten salt treatment is named STO.
[0079] Step 3: Prepare a solution with a volume ratio of H2O: N, N-dimethylformamide: ethanol of 1:1:1. Dissolve 0.216g Ni(NO3)2·6H2O, 0.216g Co(NO3)2·6H2O, 0.15g trimesic acid, and 1.5g polyvinyl pyrrolidone in 30mL of the above solution. Ultrasonicate at room temperature for 30min, and then transfer the solution to a 50mL polytetrafluoroethylene hydrothermal autoclave. Place the hydrothermal autoclave in an oven, heat at 150℃ for 10h, and cool naturally to room temperature. Wash the prepared sample, centrifuge and dry it, and name the sample NiCo-MOF.
[0080] Step 4: Disperse 100 mg of STO and 7 mg of NiCo-MOF in 5 mL of ethanol. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and the oil bath temperature is set to 80 ° C. Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction. The specific experimental parameters are: NH3 flow rate of 28 mL / min, heating rate of 5 ° C / min, heating temperature of 800 ° C, and heating time of 2 hours. The prepared sample is named 7%-MOF-STO-NH3.
[0081] Step 5: Add the 7%-MOF-STO-NH3 prepared in step 4 into pure water for photocatalytic water decomposition and hydrogen production test. The specific steps are as follows:
[0082] 1) Add 10 mg of Al-doped strontium titanate photocatalyst loaded with NiCo alloy into a reactor with a volume of 105 mL, and add deionized water with a total volume of 80 mL;
[0083] 2) Before irradiation, argon gas was purged into the reactor for 15 min to remove oxygen from the system;
[0084] 3) Turn on the magnetic stirrer and the xenon lamp.
[0085] Example 5
[0086] Step 1: Same as Example 1;
[0087] Step 2: Same as Example 1;
[0088] Step 3: Same as Example 1;
[0089] Step 4: Grind 100 mg STO and 4 mg NiCo-MOF to obtain a mixture, and then place the mixture in a tube furnace filled with ammonia for high-temperature reduction to obtain Ni, Co bimetallic alloy-strontium titanate composite photocatalyst. The specific parameters of the high-temperature reduction experiment are: NH3 flow rate of 60 mL / min, heating rate of 10℃ / min, heating temperature of 700℃, and heating time of 1.5h.
[0090] Example 6
[0091] Step 1: Same as Example 1;
[0092] Step 2: Same as Example 1;
[0093] Step 3: Same as Example 1;
[0094] Step 4: Disperse 100 mg of STO and 6 mg of NiCo-MOF in 10 mL of water. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and the temperature of the oil bath is set to 100 ° C. Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction to obtain a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst. The specific parameters of the high-temperature reduction experiment are: NH3 flow rate of 20 mL / min, heating rate of 7 ° C / min, heating temperature of 600 ° C, and heating time of 2 hours.
[0095] Example 7
[0096] Step 1: Same as Example 1;
[0097] Step 2: Same as Example 1;
[0098] Step 3: Same as Example 1;
[0099] Step 4: Disperse 100 mg of STO and 10 mg of NiCo-MOF in 7 mL of methanol. Place the suspension in a glass test tube and evaporate it in a constant temperature oil bath, and the temperature of the oil bath is set to 65 ° C. Place the above sample in a tubular furnace filled with ammonia for high-temperature reduction to obtain a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst. The specific parameters of the high-temperature reduction experiment are: NH3 flow rate of 100 mL / min, heating rate of 9 ° C / min, heating temperature of 1000 ° C, and heating time of 1 hour.
[0100] Figure 1 The X-ray diffraction (XRD) diagrams of NiCo bimetallic alloy (MOF-NH3), Al-doped strontium titanate (STO), and Al-doped strontium titanate loaded with NiCo bimetallic alloy (3%-MOF-STO-NH3). The XRD characteristic peaks of NiCo-MOF after high-temperature ammonia treatment match the characteristic peaks of Ni and Co metals, indicating that NiCo alloy can be prepared by calcining NiCo-MOF with high-temperature ammonia. The structure of strontium titanate did not change significantly before and after high-temperature ammonia treatment.
[0101] Figure 2 Figures a) and b) are scanning electron microscope (SEM) and transmission electron microscope (TEM) images of 3%-MOF-STO-NH3, which further prove that NiCo alloy is loaded on the surface of strontium titanate.
[0102] Figure 3 The photocatalytic hydrogen production rate of Al-doped strontium titanate loaded with different proportions of NiCo bimetallic alloys can be seen. When the NiCo-MOF addition amount is 3%, the catalytic activity of the catalyst is the highest, and the photocatalytic water decomposition hydrogen production rate is 979.9 μmol h -1 g -1 , with a quantum efficiency of 11.9% at 350nm.
[0103] The calculation formula for the apparent quantum efficiency AQY (%) of the photocatalytic hydrogen production reaction is:
[0104]
[0105] Figure 4 This is the stability test diagram of 3%-MOF-STO-NH3 photocatalytic hydrogen production, which shows that the catalyst has good stability.
[0106] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0107] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A method for preparing a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst, characterized in that: The following steps are involved: After Al-doped strontium titanate and a metal-organic framework containing Ni, Co bimetallics are uniformly mixed, a reduction reaction is carried out in an ammonia atmosphere to obtain a Ni, Co bimetallic alloy-strontium titanate composite photocatalyst.
2. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: Al-doped strontium titanate was prepared by a hydrothermal method and molten salt.
3. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: The molar ratio of Ni to Co in the metal-organic framework containing Ni, Co bimetallic is 1:0.1-1.
4. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: The mass ratio of Al-doped strontium titanate to the metal-organic framework containing Ni, Co bimetallic is 100 mg:1-10 mg.
5. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: The uniform mixing is carried out by grinding or dispersing the Al-doped strontium titanate and the metal-organic framework containing Ni, Co bimetallic in a solvent and then evaporating to dryness.
6. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: The ammonia flow rate is 20-100 mL / min.
7. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: The temperature of the reduction reaction is 600-1000°C and the time is 1-5h.
8. The method for preparing the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst according to claim 1, characterized in that: The temperature was raised to 600-1000°C at a heating rate of 5-10°C / min.
9. A Ni, Co bimetallic alloy-strontium titanate composite photocatalyst prepared according to the method of claims 1-8.
10. Use of the Ni, Co bimetallic alloy-strontium titanate composite photocatalyst prepared according to the method of claims 1-8 in photocatalytic hydrogen production.
Citation Information
Patent Citations
Preparation method of ternary amorphous alloy modified cellulose / strontium titanate composite photocatalyst, and applications of ternary amorphous alloy modified cellulose / strontium titanate composite photocatalyst in hydrogen production through water photolysis
CN106944154A
Method for preparing oxygen-vacancy-containing strontium titanate photocatalyst
CN107552033A
Pinniform leaf heterojunction photocatalyst and preparation method thereof
CN114100682A
Preparation method of cobalt composite cobalt-nickel alloy / nitrogen-doped graphene nano-catalyst
CN114318399A
Hydrogen generation co-catalyst, photocatalyst, method for producing hydrogen, device for producing hydrogen, and semiconductor material
WO2022270501A1
Cited By
Application of cobalt monatomic doped strontium titanate composite catalytic material in activated peracetic acid catalytic degradation of organic pollutants
CN119926408A
Strontium titanate single crystal with selectively distributed same crystal face as well as preparation method and application of strontium titanate single crystal
CN120006391A
Method for constructing a hydrophilic network modified strontium titanate photocatalyst and application thereof