Inhibitor for reverse flotation desilicication of collophanite as well as preparation method and application of inhibitor
By using a compound inhibitor of polyphosphate sulfonic acid copolymer and phosphate mixture in the antiflotation and desilase process of gum phosphate ore, combined with a high-efficiency desilase collector, the loss of fine phosphate-containing minerals is solved. The problem of this method improves the recovery rate and separation efficiency of phosphorus concentrate.
Patent Information
- Application Number
- CN202410982547.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
During the anti-flotation and desilication process of gum phosphate ore, fine-grained phosphorus-containing minerals are vulnerable to loss, and the prior art is difficult to achieve selective inhibition in a neutral-alkaline environment, resulting in low recovery of phosphorus concentrate.
Using polyphosphate sulfonic acid copolymer and phosphate mixture as inhibitors, the phosphate minerals are captured by combining in a neutral-alkaline environment and combining with a brittle foam-efficient desilicate collector to achieve phosphate minerals. Efficient separation from ganglite.
It effectively inhibits the upwelling of fine-grained phosphorus-containing minerals, improves the recovery rate of phosphorus pentoxide in phosphorus concentrate, and does not affect the fluidity of desilica foam and the capture ability of the collector.
Smart Images

Figure CN118904550A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of collophanite beneficiation, and in particular to an inhibitor for reverse flotation desiliconization of collophanite, and a preparation method and application thereof. Background Art
[0002] At present, with the progress of phosphate mining, the development value of medium and low-grade siliceous-calcium collophosphate is prominent. The quality improvement and impurity reduction of medium and low-grade siliceous-calcium collophosphate is mainly reflected in the removal of siliceous gangue and carbonate gangue, mainly by flotation method. The research on the flotation process of medium and low-grade siliceous-calcium collophosphate mainly focuses on direct-reverse flotation and double reverse flotation process.
[0003] The reverse flotation of collophanite involves two flotation systems: the reverse flotation of collophanite to remove carbonate gangue and the reverse flotation of collophanite to remove siliceous gangue. The most studied selective inhibitors of collophanite are how to selectively inhibit collophanite in the reverse flotation system of collophanite to remove carbonate gangue, such as phosphoric acid, sulfuric acid, phosphorus-sulfur mixed acid, ATMP, etc., while there are almost no public reports on the selective inhibition of collophanite in the reverse flotation system of collophanite to remove siliceous gangue.
[0004] At present, for medium and low-grade calcareous silico-phosphate ore, the silicon removal by reverse flotation of silicon-phosphate ore can be achieved by using the silicon-phosphate collector BK432 independently developed by the Mining and Metallurgical Group. However, there is a problem that fine-grained phosphorus-containing minerals are easily lost in silicon tailings. It is also difficult to reduce the phosphorus grade of silicon tailings to a reasonable level through multiple silicon-containing foam sweeping. Especially for fine-grained embedded silicon-phosphate ore, finer grinding fineness is bound to lead to the loss of more fine-grained phosphorus-containing minerals.
[0005] In order to solve the loss of fine-grained phosphorus-containing minerals during the reverse flotation desiliconization process of collophanite, a selective inhibitor of fine-grained phosphorus-containing minerals in the reverse flotation desiliconization system of collophanite in a neutral-alkaline environment is urgently needed. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide an inhibitor for the reverse flotation desiliconization of collophanite, and a preparation method and use thereof, so as to achieve selective inhibition of fine-grained phosphorus-containing minerals that are easy to float in the reverse flotation desiliconization system of collophanite in a neutral-alkaline environment, thereby improving the recovery rate of phosphorus pentoxide in the phosphate concentrate of the reverse flotation desiliconization operation of collophanite.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides an inhibitor for reverse flotation desiliconization of collophanite, the inhibitor comprising a polyphosphate ester sulfonic acid copolymer and a phosphate mixture.
[0009] The inhibitor provided by the present invention is compounded with a polyphosphate sulfonic acid copolymer and a sodium phosphate salt mixture, and can achieve selective inhibition of fine-grained phosphorus-containing minerals through a reverse flotation process in a neutral-alkaline environment, and then a brittle bubble high-efficiency desiliconization collector is used to collect silicon-containing gangue of various particle sizes, thereby achieving efficient separation of phosphorus minerals and silicon-containing gangue, and further improving the recovery rate of phosphorus pentoxide in phosphate concentrate.
[0010] As a preferred technical solution of the present invention, the molecular structure of the polyphosphate sulfonic acid copolymer includes at least one phosphate group and at least one sulfonic acid group.
[0011] As a preferred technical solution of the present invention, the phosphate mixture includes monohydrogen phosphate and dihydrogen phosphate.
[0012] Preferably, the phosphate mixture comprises, by mass percentage, 50%-70% monohydrogen phosphate and 30%-50% dihydrogen phosphate.
[0013] As a preferred technical solution of the present invention, the inhibitor comprises, by weight: 4-6 parts of polyphosphate sulfonic acid copolymer and 2-4 parts of phosphate mixture.
[0014] In a second aspect, the present invention provides a method for preparing the inhibitor as described in the first aspect, characterized in that the preparation method comprises: according to a formula, mixing a polyphosphate sulfonic acid copolymer and a phosphate mixture with water to obtain the inhibitor.
[0015] In a third aspect, the present invention provides a use of the inhibitor as described in the first aspect, wherein the use comprises using the inhibitor to perform reverse flotation desiliconization on collophanite.
[0016] As a preferred technical solution of the present invention, the use includes: mixing and stirring the collophanite slurry, the inhibitor and the desiliconization collector, and then performing reverse flotation desiliconization operation to obtain silicon tailings and phosphate concentrate.
[0017] As a preferred technical solution of the present invention, the collophanite slurry is obtained by wet grinding the collophanite ore.
[0018] Preferably, the collophanite ore comprises, by mass percentage: 2 O 5 20%-28%, SiO 2 10%-30%.
[0019] Preferably, the collophanite slurry has a slurry concentration of 20wt%-40wt%.
[0020] Preferably, the pH value of the collophanite slurry is 7-8.
[0021] Preferably, solid particles with a diameter of -0.074 mm in the collophanite slurry account for 60% to 85% of the mass of all solid particles.
[0022] As a preferred technical solution of the present invention, the mixing and stirring time is 2 min-3 min.
[0023] Preferably, the stirring speed of the mixing and stirring is 1.5m / s-2m / s.
[0024] As a preferred technical solution of the present invention, the reverse flotation desiliconization operation performs at least one roughing operation and one scavenging operation.
[0025] Preferably, the added amount of the inhibitor is 200 g / t-500 g / t.
[0026] Preferably, the addition amount of the collector BK432 is 100g / t-500g / t.
[0027] Preferably, the reverse flotation operation is a closed-circuit reverse flotation.
[0028] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0029] In the reverse flotation desiliconization operation of neutral-alkaline collophanite, a specific compound reagent is used to selectively suppress fine-grained phosphorus-containing minerals through one or more reverse flotation operations without affecting the fluidity of the desiliconized foam and the collection capacity of the desiliconized collector for silicon-containing gangue, thereby improving the recovery rate of phosphorus pentoxide in phosphate concentrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a flow chart of the use of inhibitors provided by an embodiment of the present invention;
[0031] Figure 2 This is a flow chart of reverse flotation desiliconization in Application Example 1 of the present invention.
[0032] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION
[0033] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0034] This embodiment provides an inhibitor for reverse flotation desiliconization of collophanite, wherein the inhibitor comprises a polyphosphate ester sulfonic acid copolymer and a phosphate mixture.
[0035] The molecular structure of the polyphosphate sulfonic acid copolymer includes at least one phosphate group and at least one sulfonic acid group.
[0036] In the present invention, the polyphosphate sulfonic acid copolymer is a single substance, that is, an organic substance containing a phosphate group and a sulfonic acid group and having multiple hydroxyl groups, rather than a mixture of a phosphate organic substance and a sulfonic acid organic substance. For example, the polyphosphate sulfonic acid copolymer can be selected from the commercially available JXL-107 (40%) polyphosphate sulfonic acid copolymer, or a polyphosphate sulfonic acid copolymer obtained according to a synthesis method in the art.
[0037] Wherein, the phosphate mixture includes monohydrogen phosphate and dihydrogen phosphate.
[0038] In the present invention, the monohydrogen phosphate includes soluble monohydrogen phosphate such as sodium monohydrogen phosphate and potassium monohydrogen phosphate.
[0039] In the present invention, the dihydrogen phosphate includes soluble dihydrogen phosphates such as sodium dihydrogen phosphate and potassium dihydrogen phosphate.
[0040] The phosphate mixture comprises, by mass percentage, 50%-70% monohydrogen phosphate and 30%-50% dihydrogen phosphate, which is 100% in total.
[0041] In the present invention, the mass percentage of monohydrogen phosphate in the phosphate mixture is 50%-70%, for example, it can be 50%, 52%, 54%, 56%, 60%, 62%, 64%, 66%, 68% or 70%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0042] In the present invention, the mass percentage of dihydrogen phosphate in the phosphate mixture is 30%-50%, for example, it can be 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, or 50%, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0043] The inhibitor comprises, by weight, 4 to 6 parts of a polyphosphate sulfonic acid copolymer and 2 to 4 parts of a phosphate mixture.
[0044] In the present invention, the weight percentage of the polyphosphate sulfonic acid copolymer in the inhibitor is 4-6 parts, for example, 4, 4.2, 4.4, 4.6, 4.8, 5, 5.2, 5.4, 5.6, 5.8 or 6 parts, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0045] In the present invention, the phosphate mixture in the inhibitor is 2-4 parts by weight, for example, it can be 2 parts, 2 parts, 2.2 parts, 2.4 parts, 2.6 parts, 2.8 parts, 3 parts, 3.2 parts, 3.4 parts, 3.6 parts, 3.8 parts or 4 parts, but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0046] Furthermore, this embodiment provides a method for preparing the inhibitor as described above, the preparation method comprising: according to a formula, mixing a polyphosphate ester sulfonic acid copolymer and a phosphate mixture with water to obtain the inhibitor.
[0047] Further, this embodiment provides the use of the inhibitor as described above, such as Figure 1 As shown, the use includes using the inhibitor to carry out reverse flotation desiliconization on collophanite.
[0048] The use includes: mixing and stirring the collophanite slurry, the inhibitor and the desiliconization collector, and then performing reverse flotation desiliconization operation to obtain silicon tailings and phosphate concentrate.
[0049] Wherein, the collophanite slurry is obtained by wet grinding the collophanite ore;
[0050] Wherein, the collophanite ore comprises, by mass percentage: 2 O 5 20%-28%, SiO 2 10%-30%.
[0051] In the present invention, the P in the collophanite ore 2 O 5 The mass percentage is 20%-28%, for example, it can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0052] In the present invention, the SiO 2 The mass percentage is 10%-30%, for example, it can be 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28% or 30%, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0053] Among them, the slurry concentration of the collophanite slurry is 20wt%-40wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wy%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0054] In the present invention, wt% refers to mass percentage.
[0055] The pH value of the collophanite slurry is 7-8, for example, it can be 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9 or 8, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0056] Among them, the solid particles of -0.074mm in the collophanite slurry account for 60%-85% of the mass of all solid particles, for example, it can be 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84% or 85%, etc., but are not limited to the listed values, and other values not listed within the range are also applicable.
[0057] In the present invention, -0.074 mm refers to the undersize product obtained by sieving with a 0.074 mm sieve.
[0058] The mixing and stirring time is 2 min-3 min, for example, 2 min, 2.2 min, 2.4 min, 2.6 min, 2.8 min or 3 min, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0059] Among them, the stirring speed of the mixed stirring is 1.5m / s-2m / s, for example, it can be 1.5m / s, 1.6m / s, 1.7m / s, 1.8m / s, 1.9m / s or 2m / s, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0060] The reverse flotation desiliconization operation includes at least one roughing operation and one scavenging operation.
[0061] The amount of the inhibitor added is 200 g / t-500 g / t, for example, 200 g / t, 250 g / t, 300 g / t, 350 g / t, 400 g / t, 450 g / t or 500 g / t, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0062] Among them, the addition amount of the desiliconization collector is 100g / t-500g / t, for example, it can be 100g / t, 150g / t, 200g / t, 250g / t, 300g / t, 350g / t, 400g / t, 450g / t or 500g / t, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0063] In the present invention, g / t refers to adding a corresponding mass g of flotation agents such as inhibitors and desiliconization collectors to a certain amount of silico-calcium colloidal phosphate ore. The specific mixing ratio with water can be designed according to the conventional requirements in the field, that is, the amount of g / t of flotation agents in the present invention is the mass before mixing with water.
[0064] In the present invention, the addition amount of the inhibitor and the desiliconization collector is the total addition amount in the flotation operation, rather than the single addition amount. When multiple reverse flotations are used, the segmented dosage can be adjusted according to the impurity content and experiments.
[0065] In the present invention, the desiliconization collector can be selected from conventional desiliconization collectors in the art such as BK432.
[0066] Wherein, the reverse flotation operation is a closed-circuit reverse flotation.
[0067] In the present invention, the number of times the reverse flotation operation is performed can be designed according to the content of siliceous gangue in the original collophanite ore. In multiple reverse flotations, the phosphate concentrate obtained is the in-tank product of the last roughing operation.
[0068] According to the above scheme, the colloidal phosphate is added with clean water for grinding. After grinding, the slurry flows into the stirring tank, and then the inhibitor and reverse flotation desiliconization collector are added to the stirring tank in turn for stirring and selective adsorption. The slurry-adjusted material enters the reverse flotation desiliconization system. The mineralized foam scraped out by the scraper is the silicon tailings, which is discharged and stacked after dense filter pressing. The product in the tank is desiliconized phosphate concentrate.
[0069] Furthermore, in order to illustrate the effects that can be achieved by the inhibitor provided by the present invention, an actual example is used for illustrative purposes, as follows:
[0070] Example 1
[0071] This embodiment provides an inhibitor suitable for desiliconization of collophanite by reverse flotation, wherein the inhibitor comprises, by weight, 5 parts of a polyphosphate ester sulfonic acid copolymer (commercially available JXL-107 polyphosphate ester sulfonic acid copolymer) and 3 parts of a sodium phosphate salt mixture;
[0072] In the sodium phosphate salt mixture, sodium monohydrogen phosphate accounts for 70% and sodium dihydrogen phosphate accounts for 30%;
[0073] Mix the above reagents and water according to the formula to prepare an inhibitor aqueous solution of a certain concentration for use.
[0074] Example 2
[0075] This embodiment provides an inhibitor suitable for desiliconization of collophanite by reverse flotation, wherein the inhibitor comprises, by weight, 6 parts of a polyphosphate ester sulfonic acid copolymer (commercially available JXL-107 polyphosphate ester sulfonic acid copolymer) and 2 parts of a sodium phosphate salt mixture;
[0076] In the sodium phosphate salt mixture, sodium monohydrogen phosphate accounts for 60% and sodium dihydrogen phosphate accounts for 40%;
[0077] Mix the above reagents and water according to the formula to prepare an inhibitor aqueous solution of a certain concentration for use.
[0078] Example 3
[0079] This embodiment provides a depressant suitable for reverse flotation desiliconization of collophanite, wherein the depressant comprises, by weight, 5.5 parts of a polyphosphate ester sulfonic acid copolymer (commercially available JXL-107 polyphosphate ester sulfonic acid copolymer) and 2.5 parts of a sodium phosphate mixture;
[0080] In the sodium phosphate salt mixture, sodium monohydrogen phosphate accounts for 50% and sodium dihydrogen phosphate accounts for 50%;
[0081] Mix the above reagents and water according to the formula to prepare an inhibitor aqueous solution of a certain concentration for use.
[0082] Application Example 1
[0083] This embodiment provides a use of an inhibitor suitable for desiliconization by reverse flotation of collophanite, such as Figure 2 As shown in the figure, the collophanite is a medium-low grade collophanite produced in Xingshan, Hubei. The silicon-containing minerals in the ore are mainly feldspar and quartz. 2 O 5 The mass fraction is 24.45%, SiO 2 The mass fraction is 21.37%.
[0084] (1) mixing the above collophanite ore with clean water and grinding the ore, and adjusting the slurry to control the slurry concentration to 27% and the slurry pH to 7.2 after grinding;
[0085] (2) The ore pulp obtained in step (1) is mixed with an inhibitor and then with a reverse flotation desiliconization collector BK432, and then enters a flotation machine for reverse flotation desiliconization roughing operation 1 to obtain silicon tailings 1 and phosphate concentrate 1; the phosphate concentrate 1 enters an intermediate box of a flotation machine, is mixed with an inhibitor and a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 2 to obtain silicon tailings 2 and phosphate concentrate 2;
[0086] (3) The silicon tailings 1 and silicon tailings 2 obtained in step (2) are combined and enter the reverse flotation desiliconization scavenging operation 1 to obtain silicon tailings 3 and middlings 1; the middlings 1 are returned to the roughing operation 1;
[0087] (4) The silicon tailings 3 obtained in step (3) enter the reverse flotation desiliconization scavenging operation 2 to obtain silicon tailings 4 and middlings 2; the middlings 2 are returned to the scavenging operation 1;
[0088] Phosphate concentrate 2 is the final desiliconized phosphate concentrate, and silicon tailings 4 is the final silicon tailings.
[0089] Wherein, in step (2), the amount of inhibitor used in the roughing 1 process is 240 g / t, and the amount of reverse flotation desiliconization collector added is 360 g / t; in the roughing 2 process, the amount of inhibitor used in the roughing 2 process is 120 g / t, and the amount of reverse flotation desiliconization collector added is 120 g / t;
[0090] The desiliconized phosphate concentrate P obtained in this application example 2 O 5 The mass fraction is 32.68%, SiO 2 The mass fraction is 6.78%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 91.32%.
[0091] Application Example 2
[0092] This embodiment provides a use of an inhibitor suitable for reverse flotation desiliconization of collophanite, wherein the silico-calcium collophanite is a medium-low grade collophanite produced in Yunnan, and the silicon-containing minerals in the ore are mainly quartz, mica, illite, 2 O 5 The mass fraction is 21.68%, SiO 2 The quality score is 28.37%.
[0093] (1) mixing the above collophanite ore with clean water and grinding the ore, and adjusting the slurry to control the slurry concentration to 30% and the slurry pH to 7.0 after grinding;
[0094] (2) The ore pulp obtained in step (1) is mixed with an inhibitor and then with a reverse flotation desiliconization collector BK432, and then enters a flotation machine for reverse flotation desiliconization roughing operation 1 to obtain silicon tailings 1 and phosphate concentrate 1; the phosphate concentrate 1 enters an intermediate box of a flotation machine, is mixed with an inhibitor and a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 2 to obtain silicon tailings 2 and phosphate concentrate 2; the phosphate concentrate 2 enters an intermediate box of a flotation machine, is mixed with an inhibitor and a reverse flotation desiliconization collector, and then enters a flotation machine for reverse flotation desiliconization roughing operation 3 to obtain silicon tailings 3 and phosphate concentrate 3;
[0095] (3) The silicon tailings 1, 2 and 3 obtained in step (2) are combined and enter the reverse flotation desiliconization scavenging operation 1 to obtain silicon tailings 4 and middlings 1; the middlings 1 are returned to the roughing operation;
[0096] (4) The silicon tailings 4 obtained in step (3) enter the reverse flotation desiliconization scavenging operation 2 to obtain silicon tailings 5 and middlings 2; the middlings 2 are returned to the scavenging operation 1;
[0097] Phosphate concentrate 3 is the final desiliconized phosphate concentrate, and silicon tailings 5 is the final silicon tailings.
[0098] Wherein, in step (2), the amount of inhibitor used in the roughing 1 process is 360 g / t, and the amount of reverse flotation desiliconization collector added is 300 g / t; in the roughing 2 process, the amount of inhibitor used in the roughing 2 process is 80 g / t, and the amount of reverse flotation desiliconization collector added is 80 g / t; in the roughing 3 process, the amount of inhibitor used in the roughing 3 process is 40 g / t, and the amount of reverse flotation desiliconization collector added is 40 g / t;
[0099] The desiliconized phosphate concentrate P obtained in this application example 2 O 5 The mass fraction is 33.64%, SiO 2 The mass fraction is 5.47%, desiliconized phosphate concentrate P 2 O 5 Recovery rate: 91.35%.
[0100] Application Example 3
[0101] This embodiment provides a use of an inhibitor suitable for reverse flotation desiliconization of collophanite. The silico-calcium collophanite is a medium-low-grade collophanite produced in Hubei. The silicon-containing minerals in the ore are mainly feldspar, P 2 O 5 The mass fraction is 27.43%, SiO 2 The mass fraction is 14.38%.
[0102] (1) mixing the above collophanite ore with clean water and grinding the ore, and adjusting the slurry to control the slurry concentration to 25% and the slurry pH to 7.2 after grinding;
[0103] (2) The slurry obtained in step (1) is mixed with an inhibitor and then mixed with a reverse flotation desiliconization collector BK432, and then enters a flotation machine for reverse flotation desiliconization roughing operation to obtain silicon tailings 1 and phosphate concentrate 1;
[0104] (3) The silicon tailings 1 obtained in step (2) enters the reverse flotation desiliconization scavenging operation to obtain silicon tailings 2 and middlings; the middlings are returned to the roughing operation;
[0105] Phosphate concentrate 1 is the final desiliconized phosphate concentrate, and silicon tailings 2 is the final silicon tailings.
[0106] Wherein, in step (2) roughing 1, the amount of inhibitor used is 240 g / t, and the amount of reverse flotation desiliconization collector added is 200 g / t;
[0107] The desiliconized phosphate concentrate P obtained in this application example 2 O 5 The mass fraction is 33.18%, SiO 2 The mass fraction is 5.47%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 93.38%.
[0108] Application Example 4
[0109] The only difference from Application Example 3 is that no inhibitor is added during the reverse flotation process.
[0110] The phosphate concentrate P obtained in this application example 2 O 5 The mass fraction is 32.48%, SiO 2 The mass fraction is 7.12%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 88.36%.
[0111] Application Example 5
[0112] The only difference from Application Example 3 is that the sodium phosphate salt mixture in the depressant used in the reverse flotation process is replaced by an equal amount of sodium hexametaphosphate.
[0113] The final P obtained in this application example 2 O 5 The mass fraction is 29.37%, SiO 2 The mass fraction is 11.58%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 85.37%.
[0114] Application Example 6
[0115] The only difference from Application Example 3 is that the polyphosphate sulfonic acid copolymer in the depressant used in the reverse flotation process is replaced by an equal amount of sodium lignin sulfonate.
[0116] The final P obtained in this application example 2 O 5 The mass fraction is 31.47%, SiO 2 The mass fraction is 10.68%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 83.67%, and the desiliconized foam in the flotation process tends to become sticky.
[0117] Application Example 7
[0118] The only difference from Application Example 3 is that the phosphate mixture is replaced by an equal amount of sodium monohydrogen phosphate.
[0119] The final P obtained in this application example 2 O 5 The mass fraction is 31.23%, SiO 2 The mass fraction is 8.25%, desiliconized phosphate concentrate P 2 O 5 Recovery rate: 87.15%.
[0120] Application Example 8
[0121] The only difference from Application Example 3 is that the phosphate mixture is replaced by an equal amount of sodium dihydrogen phosphate.
[0122] The final P obtained in this application example 2 O 5 The mass fraction is 31.27%, SiO 2 The mass fraction is 7.86%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 86.21%.
[0123] Application Example 9
[0124] The only difference from Application Example 3 is that the sodium dihydrogen phosphate in the phosphate mixture is replaced by an equal amount of sodium phosphate Na 3 PO 4 .
[0125] The final P obtained in this application example 2 O 5 The mass fraction is 30.37%, SiO 2 The mass fraction is 9.57%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 87.37%.
[0126] Application Example 10
[0127] The only difference from Application Example 3 is that the polyphosphate ester sulfonic acid copolymer in the phosphate mixture is replaced by C3-9 alkyl phosphate (CAS: 68515-98-0) and sodium lignin sulfonate in a mass ratio of 1:1.
[0128] The final P obtained in this application example 2 O 5 The mass fraction is 29.25%, SiO 2 The mass fraction is 10.37%, desiliconized phosphate concentrate P 2 O 5 The recovery rate is 84.37%.
[0129] It can be seen from the results of the above embodiments and application examples that the composite collector provided by the present invention can achieve selective inhibition of phosphorus-containing minerals, especially fine-grained phosphorus-containing minerals, in the reverse flotation desiliconization operation of neutral-alkaline collophanite, and further, does not affect the fluidity of the reverse flotation desiliconization foam and the collection capacity of the reverse flotation desiliconization collector for silicon-containing gangue. Furthermore, the effective recovery of fine-grained phosphorus-containing minerals is achieved, and the total recovery rate of phosphorus pentoxide in phosphate concentrate is improved.
[0130] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0131] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0132] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0133] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A depressant for desiliconization of collophanite by reverse flotation, characterized in that: The inhibitors include polyphosphate ester sulfonic acid copolymers and phosphate mixtures.
2. The inhibitor according to claim 1, characterized in that The molecular structure of the polyphosphate sulfonic acid copolymer includes at least one phosphate group and at least one sulfonic acid group.
3. The inhibitor according to claim 1, characterized in that The phosphate mixture includes monohydrogen phosphate and dihydrogen phosphate; Preferably, the phosphate mixture comprises, by mass percentage, 50%-70% monohydrogen phosphate and 30%-50% dihydrogen phosphate.
4. The inhibitor according to claim 1, characterized in that The inhibitor comprises, by weight: 4 to 6 parts of a polyphosphate sulfonic acid copolymer and 2 to 4 parts of a phosphate mixture.
5. The method for preparing the inhibitor according to any one of claims 1 to 4, characterized in that: The preparation method comprises: mixing a polyphosphate sulfonic acid copolymer, a phosphate mixture and water according to a formula to obtain an inhibitor.
6. A use of the inhibitor according to any one of claims 1 to 4, characterized in that: The use includes using the inhibitor to carry out reverse flotation desiliconization on collophanite.
7. The use according to claim 6, characterized in that The use includes: mixing and stirring the collophanite slurry, the inhibitor and the desiliconization collector, and then performing reverse flotation desiliconization operation to obtain silicon tailings and phosphate concentrate.
8. The use according to claim 7, characterized in that The collophanite slurry is obtained by wet grinding the raw collophanite ore; Preferably, the collophanite ore comprises, by mass percentage, P2O5 20%-28%, SiO2 10%-30%; Preferably, the collophanite slurry has a slurry concentration of 20wt%-40wt%; Preferably, the pH value of the collophanite slurry is 7-8; Preferably, solid particles with a diameter of -0.074 mm in the collophanite slurry account for 60% to 85% of the mass of all solid particles.
9. The use according to claim 7, characterized in that: The mixing time is 2-3 minutes; Preferably, the stirring speed of the mixing and stirring is 1.5m / s-2m / s.
10. The use according to claim 7, characterized in that: The reverse flotation desiliconization operation is performed by at least one roughing operation and one scavenging operation; Preferably, the inhibitor is added in an amount of 200 g / t-500 g / t; Preferably, the addition amount of the collector BK432 is 100g / t-500g / t; Preferably, the reverse flotation operation is a closed-circuit reverse flotation.