Stud bolt large chamfer cold heading forming process and mold

Through the combination of multi-station cold heading machine and special mold, the large chamfer of double-head bolts is gradually formed, which solves the problems of manual impact and mold damage, and achieves efficient and stable production of large chamfered bolts.

CN118905136APending Publication Date: 2024-11-08CHONGQING STANDARD FASTNERS IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411344147.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the processing quality and production capacity of large chamfered double-head bolts are greatly affected by manual factors, and traditional processing methods cause mold damage, making it difficult to efficiently produce large chamfered double-head bolts.

Method used

Using a multi-station cold heading machine and a special mold combination, the cold heading forming steps of one, two and three sequences gradually form large chamfers to control the force of the mold, avoid excessive deformation and fracturing, and directly form large inverts. Angle bolts reduce lathe processing needs.

Benefits of technology

It improves the processing efficiency and production capacity of large chamfers of double-head bolts, extends the service life of the mold, reduces manual intervention and lathe processing waste, and achieves efficient and stable production of large chamfers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905136A_ABST
    Figure CN118905136A_ABST
Patent Text Reader

Abstract

The invention relates to the field of new energy automobile part production, and discloses a stud bolt large chamfer cold heading forming process and a stud bolt large chamfer cold heading forming die, through the improvement of the process and the die, one end of a rod material is firstly pre-chamfered and the rod diameter is controlled in the first procedure, the other end of the rod material is shrunk in the second procedure, and then two ends are synchronously upset, formed and chamfered in the third procedure. According to the cold heading process, a stud bolt product with the end chamfer width larger than 5 mm can be directly machined and formed through the cold heading process, and the problem that in the prior art, a large chamfer of a stud bolt is formed through turning, and the machining quality and the productivity are greatly affected by artificial factors can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new energy automobile parts production, and in particular to a cold heading forming process and a die for a stud bolt with a large chamfer. Background Art

[0002] New energy vehicles represent the future development direction of the automotive industry. They not only help reduce environmental pollution and improve energy efficiency, but also bring a more economical and smarter driving experience. With the continuous advancement of technology and continued policy support, the market share of new energy vehicles will continue to grow and become one of the mainstream means of transportation. Stud chamfered bolts are required in battery packs, motors, reducers, suspension systems, transmission systems and body connections in new energy vehicles. The chamfer design of stud chamfered bolts can facilitate alignment and insertion, improve assembly efficiency, and disperse stress, reduce local stress concentration during tightening, and improve connection reliability.

[0003] According to GB / T 901-2000 "Studs", GB / T 3103.1-2000 "Fastener Tolerances Bolts, Screws and Studs", GB / T According to the general standards such as GB / T 1231-2006 "Technical Conditions for High-Strength Large Hexagon Head Bolts, Large Hexagon Nuts and Washers for Steel Structures" and GB / T 3098.1-2010 "Mechanical Properties of Fasteners - Bolts, Screws and Studs", the chamfer size of the bolt head is usually (1mm×45°) or (2mm×45°), and the chamfer width is usually 1-2mm. During production, the stud bolts with such chamfers are firstly cold-forged at both ends after cutting to reduce the rod diameter. In the second process, the two ends after the rod is shrunk are directly cold-forged and chamfered through the die. Because the chamfer size is small and the deformation of the rod end is small during the forging process, the rod end after the diameter reduction can be easily forged by cold forging without causing damage to the die and cold forging equipment.

[0004] However, there is a need for a large chamfered stud bolt, one end of which has a chamfer width of 5mm, which is much larger than that of conventional bolts and exceeds the requirements of current standards. It is a non-standard product. Conventional technology is still used to form this large chamfer, which requires a far greater upsetting pressure than the conventional one to deform the end of the rod. At the same time, the upsetting pressure on the mold is very likely to cause fracturing damage to the mold, so there is no mature processing technology for this bolt product in the prior art. Now, the rod can only be shrunk by conventional technology and then clamped on a lathe to form a large chamfer with a width of 5mm. However, only one workpiece can be clamped for processing at a time, and clamping takes a lot of time to ensure the processing accuracy of different products in the batch processing process. The efficiency of a single processing is low. To ensure production capacity, workers need high-intensity labor. In this way, the processing quality and production capacity of the product are greatly affected by human factors, which to a certain extent limits the supply of large chamfered stud bolt products. Summary of the invention

[0005] The present invention aims to provide a cold heading forming process for stud bolts with large chamfers, so as to solve the problem in the prior art that the stud bolts with large chamfers are formed by turning, and the processing quality and production capacity are greatly affected by human factors.

[0006] To achieve the above object, the present invention adopts the following technical solution: a large chamfer cold heading forming process of stud bolts, comprising the following steps:

[0007] A. Cutting: Cut the coil steel into rods of a certain length, the diameter of which is 97% of the outer diameter of the stud bolt;

[0008] B. One sequence: Use one sequence of lower die to cold forge the lower end of the bar material on a multi-station cold forging machine to form a large chamfer of the blank. The width of the large chamfer of the blank is 120% of the width of the formed large chamfer. The diameter of the small end of the large chamfer of the blank is the forming size. Keep the diameter of the bar material unchanged during the one sequence;

[0009] C. Second order: Use the second order upper die to shrink the upper section of the rod material after the first order processing and form a chamfer at the upper end. In the process, keep the large chamfer of the blank from deformation;

[0010] D. Three-step process: Use the two-step upper die to keep the upper section and upper end of the rod material from deformation, use the three-step lower die to shrink the lower section of the rod material after the two-step processing, and press the large chamfer of the blank into a formed large chamfer.

[0011] Preferably, as an improvement, in step B, a punch is used on a multi-station cold heading machine to punch the rod material into a first-order lower die to complete a first-order forming. A frustum is provided at the end of the punch, and the diameter of the frustum is 50%-60% of the diameter of the rod material. The height of the frustum is consistent with the large chamfer width of the blank.

[0012] Preferably, as an improvement, in step C, the upper section of the rod material is shrunk to 92%-93% of the outer diameter of the stud bolt, and the diameter of the lower section of the rod material is upset to 1.01 times the outer diameter of the stud bolt.

[0013] Preferably, as an improvement, in step C, the length of the rod material is controlled to be 1.02 times the length of the stud bolt.

[0014] Preferably, as an improvement, in step D, the diameter of the lower section of the rod material is controlled to be 93%-94% of the diameter of the stud bolt.

[0015] The principle and advantages of this scheme are as follows: in actual application, the diameter of the rod material is controlled during the blanking process, and the deformation is reserved for the subsequent deformation of the first and second sequences. Then, in the first sequence, the new design of the mold and the special punching needle are used to form a large chamfer of the blank with a deformation margin at the end without changing the diameter of the rod material. In this way, the radial pressure on the mold is small, and the structural design of the punching needle enables the large chamfer of the blank with a width of more than 5mm to be smoothly formed; then, after the second sequence, the end contacted by the punching needle in the first sequence is retracted, and the pit formed by the punching needle in the first sequence at the end of the rod material is flattened during the retracting process. At the same time, the large chamfer of the blank at the other end remains unchanged, and the rod diameter is slightly increased. In this way, the radial force received by the second sequence upper die as a rod retracting die is controllable, and it is not easy to cause damage to the second sequence die, and the rod retracting forming of the end of the rod material is easy. Then, the two ends are retracted and the chamfers are corrected to the final size through the third sequence. The deformation of the third sequence is relatively smaller, and it can be smoothly formed during the cold heading process, and it will not exert excessive pressure on the die, which can avoid damage to the die. Compared with the traditional cold forging process for stud bolts, this cold forging process can effectively form large chamfers with a width greater than 5mm on the bolt head while ensuring the service life of the mold, and can effectively avoid mold damage caused by excessive upsetting pressure required for large deformation. Compared with the method of cold forging the shrink rod and then turning it, this solution directly forms it through cold forging, and does not need to be manually loaded on the lathe for machining again. It has higher production efficiency and higher utilization rate of raw materials, reducing the waste caused by turning iron chips.

[0016] The cold heading forming die for stud bolts with large chamfers is used to complete the above-mentioned cold heading forming process for stud bolts with large chamfers, and includes a first-order lower die, a second-order upper die, a second-order lower die and a third-order lower die. The first-order lower die, the second-order upper die, the second-order lower die and the third-order lower die all include a die core and a die sleeve. The die core is made of carbide steel, and the die sleeve is made of tool steel with a hardness of 44-48HRC.

[0017] Preferably, as an improvement, the interference between the mold core and the mold sleeve is 0.3%-0.5% of the actual outer diameter of the mold core.

[0018] Preferably, as an improvement, the core roughness of the first-order lower mold is 0.4, the core of the first-order lower mold is provided with a penetrating first-order forming hole, the first-order forming hole includes an ejector hole and a first-order transition hole, and a conical first-order chamfered hole is connected between the ejector hole and the first-order transition hole.

[0019] Preferably, as an improvement, the second-order lower mold has the same structure as the first-order lower mold, but the length of the second-order transition hole of the second-order lower mold is smaller than the length of the first-order transition hole, and the mold core of the second-order upper mold is provided with a penetrating second-order forming hole, and the second-order forming hole includes a pin hole, a second-order shrinkage rod hole and a second-order transition hole arranged in sequence from top to bottom.

[0020] Preferably, as an improvement, the mold core of the three-sequence lower mold is provided with a through three-sequence forming hole, and the three-sequence forming hole includes a three-sequence transition hole, a three-sequence forming hole, a three-sequence chamfering hole and an ejector hole arranged in sequence from top to bottom.

[0021] The principles and advantages of this solution are as follows: in actual application, the materials of the mold core and the mold sleeve are both made of high-strength materials. During assembly, the connection between the mold core and the mold sleeve is stable by controlling the interference fit. The first-order lower mold is used to first form a large chamfer of the blank at one end of the rod material. The control of its roughness ensures that the rod material can deform smoothly after being pressed, and no surface scratches will be formed. The diameter of the first-order forming hole of the first-order lower mold is the same as the diameter of the rod material, which limits the radial deformation of the rod material during the first-order process, thereby ensuring that the end of the rod material can effectively form a large chamfer of the blank in the first-order chamfer hole. The length design of the second-order transition hole of the second-order lower mold enables the upper end of the rod material to effectively complete the rod shrinkage in the second-order upper mold during the second-order processing. The diameter of the ejector hole in the second-order upper mold is the same as the rod diameter after the rod material is shrunk, and a flat-head ejector is used to correct the pit left at the end of the rod material after the first-order processing while completing the rod shrinkage in the second-order process. The three-sequence lower die is equipped with a three-sequence upper die. Similar to the synchronous cold heading chamfering of both ends of conventional stud bolts, the three-sequence lower die and the three-sequence upper die synchronously cold head the rod material that has been shrunk at one end and formed with a large chamfer of the blank at the other end, so that the end of the shrunk rod forms a conventional chamfer, while the end of the blank with a large chamfer completes the forming of the large chamfer while the rod is shrunk. Such a die combination, combined with the corresponding cold heading forming process, can directly cold head the large chamfer of the stud bolt. The die structure is reasonably designed and is not easily damaged during use. It can produce and process large chamfer stud bolts for a long time to meet production needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the deformation of the rod material during the processing in Example 1 of the present invention.

[0023] Figure 2 This is a schematic structural diagram of a first-order lower die and a punch in Example 2 of the present invention.

[0024] Figure 3 This is a schematic diagram of the structure of the second-order mold in Example 2 of the present invention.

[0025] Figure 4 This is a schematic diagram of the structure of the three-sequence lower mold in Example 2 of the present invention. DETAILED DESCRIPTION

[0026] The following is further described in detail through specific implementation methods:

[0027] The figure marks in the drawings of the specification include: mold sleeve 1, mold core 2, punch pin 3, round table 4, first-order transition hole 5, first-order chamfering hole 6, ejector hole 7, second-order lower mold 8, second-order upper mold 9, second-order shrink rod hole 10, second-order transition hole 11, third-order transition hole 12, third-order forming hole 13, and third-order chamfering hole 14.

[0028] Embodiment 1, a cold heading forming process for stud bolts with large chamfers, comprising the following steps:

[0029] A. Cutting: Cut the coil steel into rods of a certain length, the diameter of which is 97% of the outer diameter of the stud bolt;

[0030] B. One sequence: on a multi-station cold heading machine, a punching needle 3 is used to punch the bar into the first sequence lower die to complete the first sequence forming. A round table 4 is provided at the end of the punching needle 3. The diameter of the round table 4 is 50%-60% of the diameter of the bar. The height of the round table 4 is consistent with the width of the large chamfer of the blank. The first sequence lower die forms a large chamfer of the blank at the lower end of the bar. The width of the large chamfer of the blank is 120% of the width of the large chamfer. The diameter of the small end of the large chamfer of the blank is the forming size. The diameter of the bar remains unchanged during the first sequence;

[0031] C. Second order: Use the second order upper die 9 to shrink the upper section of the rod material after the first order processing and form a chamfer at the upper end. During the process, keep the large chamfer of the blank from deformation. The upper section of the rod material is shrunk to 92%-93% of the outer diameter of the stud bolt, and the diameter of the lower section of the rod material is upset to 1.01 times the outer diameter of the stud bolt. The length of the rod material is controlled to be 1.02 times the length of the stud bolt.

[0032] D. Three steps: Use the two-step upper die 9 to keep the upper section and upper end of the rod material from deformation, and use the three-step lower die to shrink the lower section of the rod material after the two-step processing, control the diameter of the lower section of the rod material to 93%-94% of the diameter of the stud bolt, and press the large chamfer of the blank into a formed large chamfer.

[0033] In the specific implementation process, the diameter of the rod material is controlled during the blanking process to reserve deformation for the subsequent first and second order deformations. Then, in the first order, the new design of the mold and the dedicated punch 3 are used, such as Figure 1As shown, without changing the diameter of the rod, a large chamfer of the blank with a deformation margin is first formed at the end. In this way, the radial pressure on the mold is small, and the structural design of the punch 3 allows the large chamfer of the blank with a width of more than 5mm to be smoothly formed; then through the second sequence, the end that the punch 3 contacts in the first sequence is shrunk, and the pit formed by the punch 3 in the first sequence at the end of the rod is flattened during the rod shrinking process. At the same time, the large chamfer of the blank at the other end remains unchanged, and the rod diameter is slightly increased. In this way, the radial force on the second sequence upper die 9 as a rod shrinking die is controllable, and it is not easy to cause damage to the second sequence die, and the rod end is easy to shrink. Then, through the third sequence, the two ends are shrunk and the chamfers are corrected to the final size. The deformation of the third sequence is relatively smaller, and it can be smoothly formed during the cold heading process, and it will not exert too much pressure on the mold, which can avoid damage to the mold. Compared with the traditional cold forging process for stud bolts, this cold forging process can effectively form large chamfers with a width greater than 5mm on the bolt head while ensuring the service life of the mold, and can effectively avoid mold damage caused by excessive upsetting pressure required for large deformation. Compared with the method of cold forging the shrink rod and then turning it, this solution directly forms it through cold forging, and does not need to be manually loaded on the lathe for machining again. It has higher production efficiency and higher utilization rate of raw materials, reducing the waste caused by turning iron chips.

[0034] Embodiment 2, a cold heading forming mold for stud bolts with large chamfers, is applied to the cold heading forming process for stud bolts with large chamfers in Embodiment 1, and includes a first-order lower die, a second-order upper die 9, a second-order lower die 8 and a third-order lower die. The first-order lower die, the second-order upper die 9, the second-order lower die 8 and the third-order lower die all include a die core 2 and a die sleeve 1. The die core 2 is cemented carbide steel, and the die sleeve 1 is tool steel with a hardness of 44-48HRC. The interference between the die core 2 and the die sleeve 1 is 0.3%-0.5% of the actual outer diameter of the die core 2.

[0035] like Figure 2 As shown, the roughness of the core 2 of the first-order lower die is 0.4, and the core 2 of the first-order lower die is provided with a through first-order forming hole, and the first-order forming hole includes an ejector hole 7 and a first-order transition hole 5, and a conical first-order chamfering hole 6 is connected between the ejector hole 7 and the first-order transition hole 5, and the first-order lower die is equipped with a punching needle 3, and a frustum 4 is provided at the end of the punching needle 3, and the diameter of the frustum 4 is 50%-60% of the diameter of the rod material, and the height of the frustum 4 is consistent with the large chamfer width of the blank.

[0036] like Figure 3 As shown, the second-order lower mold 8 has the same structure as the first-order lower mold, but the length of the second-order transition hole 11 of the second-order lower mold 8 is smaller than the length of the first-order transition hole 5, and the mold core 2 of the second-order upper mold 9 is provided with a penetrating second-order forming hole, and the second-order forming hole includes a pin hole 7, a second-order shrinkage rod hole 10 and a second-order transition hole 11 arranged in sequence from top to bottom.

[0037] like Figure 4As shown, the mold core 2 of the three-sequence lower mold is provided with a through three-sequence forming hole 13, and the three-sequence forming hole 13 includes a three-sequence transition hole 12, a three-sequence forming hole 13, a three-sequence chamfering hole 14 and an ejector hole 7 which are arranged in sequence from top to bottom.

[0038] During the specific implementation process, the materials of the mold core 2 and the mold sleeve 1 are both selected from materials with relatively high strength. During assembly, the connection between the mold core 2 and the mold sleeve 1 is ensured to be stable by controlling the interference fit. The first-order lower mold is used to first form a large chamfer of the blank at one end of the rod material. The control of its roughness ensures that the rod material can deform smoothly after being pressed, and no surface scratches will be formed. The diameter of the first-order forming hole of the first-order lower mold is the same as the diameter of the rod material, which limits the radial deformation of the rod material during the first-order process, thereby ensuring that the end of the rod material can effectively form a large chamfer of the blank in the first-order chamfer hole 6. The length design of the second-order transition hole 11 of the second-order lower mold 8 enables the upper end of the rod material to effectively complete the rod shrinking in the second-order upper mold 9 during the second-order processing. The diameter of the ejector hole 7 in the second-order upper mold 9 is the same as the rod diameter after the rod material is shrunk, and a flat-head ejector is used to correct the pit left at the end of the rod material after the first-order processing while completing the rod shrinking in the second-order process. The three-sequence lower die is equipped with a three-sequence upper die. Similar to the synchronous cold heading chamfering of both ends of conventional stud bolts, the three-sequence lower die and the three-sequence upper die synchronously cold head the rod material that has been shrunk at one end and formed with a large chamfer of the blank at the other end, so that the end of the shrunk rod forms a conventional chamfer, while the end of the blank with a large chamfer completes the forming of the large chamfer while the rod is shrunk. Such a die combination, combined with the corresponding cold heading forming process, can directly cold head the large chamfer of the stud bolt. The die structure is reasonably designed and is not easily damaged during use. It can produce and process large chamfer stud bolts for a long time to meet production needs.

[0039] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. The process of cold heading with large chamfer of stud bolts is characterized by: The following steps are involved: A. Cutting: Cut the coil steel into rods of a certain length, the diameter of which is 97% of the outer diameter of the stud bolt; B. One sequence: Use one sequence of lower die to cold forge the lower end of the bar material on a multi-station cold forging machine to form a large chamfer of the blank. The width of the large chamfer of the blank is 120% of the width of the formed large chamfer. The diameter of the small end of the large chamfer of the blank is the forming size. Keep the diameter of the bar material unchanged during the one sequence; C. Second order: Use the second order upper die to shrink the upper section of the rod material after the first order processing and form a chamfer at the upper end. In the process, keep the large chamfer of the blank from deformation; D. Three-step process: Use the two-step upper die to keep the upper section and upper end of the rod material from deformation, use the three-step lower die to shrink the lower section of the rod material after the two-step processing, and press the large chamfer of the blank into a formed large chamfer.

2. The process for cold heading of stud bolts with large chamfers according to claim 1, characterized in that: In step B, a punch is used on a multi-station cold heading machine to punch the rod into a lower die to complete a first-order forming. A frustum is provided at the end of the punch. The diameter of the frustum is 50%-60% of the diameter of the rod, and the height of the frustum is consistent with the large chamfer width of the blank.

3. The process for cold heading of stud bolts with large chamfers according to claim 2, characterized in that: In step C, the upper section of the rod material is shrunk to 92%-93% of the outer diameter of the stud bolt, and the diameter of the lower section of the rod material is upset to 1.01 times the outer diameter of the stud bolt.

4. The process for cold heading of stud bolts with large chamfers according to claim 3 is characterized in that: In step C, the length of the rod material is controlled to be 1.02 times the length of the stud bolt.

5. The process for cold heading of stud bolts with large chamfers according to claim 4, characterized in that: In step D, the diameter of the lower section of the rod material is controlled to be 93%-94% of the diameter of the stud bolt.

6. Stud bolt large chamfer cold heading forming die, characterized by: Used to complete any one of claims 1-5 of cold heading forming processes for stud bolts with large chamfers, comprising a first-order lower die, a second-order upper die, a second-order lower die and a third-order lower die, wherein the first-order lower die, the second-order upper die, the second-order lower die and the third-order lower die all comprise a die core and a die sleeve, wherein the die core is made of carbide steel, and the die sleeve is made of tool steel with a hardness of 44-48HRC.

7. The large chamfer cold heading forming die for stud bolts according to claim 6, characterized in that: The interference between the mold core and the mold sleeve is 0.3%-0.5% of the actual outer diameter of the mold core.

8. The cold heading forming die for stud bolts with large chamfers according to claim 7, characterized in that: The core roughness of the first-order lower mold is 0.4, and the core of the first-order lower mold is provided with a penetrating first-order forming hole, the first-order forming hole includes an ejector hole and a first-order transition hole, and a conical first-order chamfered hole is connected between the ejector hole and the first-order transition hole.

9. The cold heading forming die for stud bolts with large chamfers according to claim 8, characterized in that: The second-order lower mold has the same structure as the first-order lower mold, but the length of the second-order transition hole of the second-order lower mold is smaller than that of the first-order transition hole. The mold core of the second-order upper mold is provided with a penetrating second-order forming hole, and the second-order forming hole includes a pin hole, a second-order shrinkage rod hole and a second-order transition hole which are arranged in sequence from top to bottom.

10. The cold heading forming die for stud bolts with large chamfers according to claim 9, characterized in that: The mold core of the three-sequence lower mold is provided with a penetrating three-sequence forming hole, and the three-sequence forming hole includes a three-sequence transition hole, a three-sequence forming hole, a three-sequence chamfering hole and an ejector hole which are arranged in sequence from top to bottom.

Citation Information

Patent Citations

  • Process for manufacturing quincuncial dowel screws

    CN102601589A

  • Bolt large chamfering cold heading die and process

    CN108787979A

  • Double-end bolt cold heading integrated forming device

    CN213410224U

  • Cold heading supporting head bolt die

    CN215544631U

  • Method for making bolts with high neck

    RU2110352C1