Aluminum-based composite powder and preparation method thereof as well as aluminum-based composite material and preparation method thereof
Through the step-by-step methods of mechanical powder mixing, plasma spheroidization treatment and heat treatment, the problem of nanoparticle agglomeration is solved, the mechanical properties of aluminum-based composite materials are improved, the uniform distribution and efficient addition of ceramic nanoparticles are achieved, and the strength of the material is improved. and resilience.
Patent Information
- Application Number
- CN202410990760.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-23
AI Technical Summary
During the preparation of aluminum-based composite materials, nanoparticles are prone to agglomeration, resulting in a decrease in material strength and weakening of toughness, and insufficient effective addition of nanoparticles, affecting material performance.
Using the step-by-step method of mechanical powder mixing, plasma spheroidization treatment and heat treatment, the amount of ceramic nanoparticles is gradually increased, and the nanoparticles are integrated into the aluminum matrix through high-temperature melting and surface tension. The crystal structure is improved, and the agglomeration is avoided. Repeat the above steps until the target addition amount is reached.
It effectively improves the distribution uniformity of ceramic nanoparticles in aluminum-based raw materials, avoids agglomeration, increases the amount of nanoparticles, improves the mechanical properties of aluminum-based composite materials, and obtains high-strength, high toughness, and high stiffness materials.
Smart Images

Figure CN118905212A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of aluminum-based composite materials, and in particular to an aluminum-based composite powder and a preparation method thereof, an aluminum-based composite material and a preparation method thereof. Background Art
[0002] The core component of aluminum-based composite materials lies in the nanoparticles evenly distributed inside the aluminum matrix. When these nanoparticles are embedded in the aluminum matrix in a dispersed state, they can effectively hinder the dislocation movement inside the crystal, thereby significantly enhancing the overall strength of the alloy.
[0003] In the related art, the raw powder of aluminum-based composite materials is usually prepared by mechanical powder mixing, that is, nanoparticles are introduced into the aluminum powder system by mechanical vibration to achieve full mixing of the two. However, in actual operation, nanoparticles are very prone to agglomeration due to their high specific surface area and surface energy. The agglomeration of nanoparticles not only fails to play its due strengthening role, but also easily causes stress concentration, and ultimately reduces the toughness of aluminum-based composite materials.
[0004] The above contents are only used to assist in understanding the technical solution of the present application and do not constitute an admission that the above contents are prior art. Summary of the invention
[0005] The main purpose of the present application is to provide an aluminum-based composite powder and a preparation method thereof, an aluminum-based composite material and a preparation method thereof, aiming to solve the technical problem that nanoparticles are easy to agglomerate during the preparation of aluminum-based composite powder.
[0006] To achieve the above object, the present invention provides a method for preparing an aluminum-based composite powder, which comprises the following steps:
[0007] Mechanically mixing the aluminum-based raw material and a portion of the ceramic nanoparticles to obtain a first composite powder;
[0008] performing plasma spheroidization treatment on the first composite powder to obtain a second composite powder;
[0009] heat treating the second composite powder to obtain a third composite powder;
[0010] In the case where the current total amount of the ceramic nanoparticles added is less than the target total amount, the third composite powder is used as the aluminum-based raw material, and the step of mechanically mixing the aluminum-based raw material and part of the ceramic nanoparticles is returned to be executed until the current total amount of the ceramic nanoparticles added is equal to the target total amount, and the third composite powder is determined as an aluminum-based composite powder, wherein the target total amount of the ceramic nanoparticles added is 2 to 8 wt.%, and the single amount of the ceramic nanoparticles added is less than 2 wt.%.
[0011] In one embodiment, the ceramic nanoparticles include at least one of TiN, TiC, SiC and TiB2.
[0012] In one embodiment, the aluminum-based raw material that is initially mechanically mixed with the ceramic nanoparticles is selected from aluminum alloy powder;
[0013] In terms of mass percentage, the aluminum alloy powder comprises: 2-6% Mn, 0.5-1% Sc, and the remainder Al; or,
[0014] In terms of mass percentage, the aluminum alloy powder includes: 2-6% Mn, 0.1-5% Mg, 0.5-1% Sc, 0.1-0.5% Zr, and the rest is Al.
[0015] In one embodiment, the particle size of the aluminum alloy powder is 15 to 53 μm;
[0016] And / or, the particle size of the ceramic nanoparticles is 10 to 50 nm.
[0017] In one embodiment, the mechanical powder mixing includes: ultrasonic vibration powder mixing, and the powder mixing time is 10 to 30 minutes.
[0018] In one embodiment, the powder feeding rate of the plasma spheroidization treatment is 30 to 100 g / min;
[0019] and / or, the reaction chamber pressure of the plasma spheroidization treatment is 13 to 18 psi;
[0020] And / or, the power of the plasma spheroidization treatment is 30 to 50 KW;
[0021] and / or, the flow rate of the central gas argon gas in the plasma spheroidization treatment is 15 to 25 slpm;
[0022] and / or, the flow rate of the sheath gas argon gas in the plasma spheroidization treatment is 45 to 60 slpm;
[0023] And / or, the flow rate of the carrier gas in the plasma spheroidization treatment is 2 to 5 slpm.
[0024] In one embodiment, the heat treatment temperature is 400-500° C., and the heat preservation time is 2-6 hours.
[0025] The embodiment of the present application also provides an aluminum-based composite powder, which is prepared by the above method.
[0026] The present invention also provides a method for preparing an aluminum-based composite material, which comprises the following steps:
[0027] Providing an aluminum-based composite powder, wherein the aluminum-based composite powder is prepared by the above method;
[0028] The aluminum-based composite powder is subjected to selective laser melting treatment to obtain an aluminum-based composite material.
[0029] An embodiment of the present application also provides an aluminum-based composite material, which includes an aluminum-based composite powder prepared by the above-mentioned aluminum-based composite powder preparation method, or an aluminum-based composite material prepared by the above-mentioned aluminum-based composite material preparation method.
[0030] The embodiment of the present application discloses a method for preparing aluminum-based composite powder, wherein a first composite powder is obtained by mechanically mixing aluminum-based raw materials with ceramic nanoparticles accounting for a portion of the total amount of target addition. Then, the first composite powder is subjected to plasma spheroidization treatment, and the ceramic nanoparticles on the surface of the aluminum-based raw materials absorb heat and melt rapidly by means of the high temperature of the plasma, thereby being integrated into the matrix of the aluminum-based raw materials; at the same time, the powder is condensed into spherical droplets under the action of surface tension, and these spherical droplets solidify after cooling, thereby obtaining spherical particles with strong fluidity and dense packing (i.e., the second composite powder). Then, the second composite powder is subjected to heat treatment; due to the extremely short melting and solidification time in the plasma spheroidization treatment, the morphology of the ceramic nanoparticles in the second composite powder is not very stable, and heat treatment can just change the crystal structure of the material in the powder; the reorganization of this crystal structure helps to eliminate defects and stresses inside the material, thereby improving the overall stability of the material and preventing it from agglomerating with newly added particles in the next round of plasma spheroidization treatment, so as to obtain a third composite powder. Then, the third composite powder is used as the aluminum-based raw material again, and the above-mentioned steps of mechanical powder mixing, plasma spheroidization treatment and heat treatment are repeated until the amount of ceramic nanoparticles added reaches its target total amount, thereby obtaining an aluminum-based composite powder. The aluminum-based composite powder prepared by the above-mentioned step-by-step addition of ceramic nanoparticles, and repeated execution of the steps of mechanical powder mixing, plasma spheroidization treatment and heat treatment has a smooth surface and a regular spherical shape, and can effectively improve the distribution uniformity of ceramic nanoparticles in the aluminum-based raw material, avoid the problem of agglomeration caused by adding a large amount of ceramic nanoparticles at one time, and the difficulty of plasma spheroidization treatment, and increase the effective amount of ceramic nanoparticles added in the aluminum alloy composite powder. In the further application process of the aluminum-based composite powder, the aluminum-based composite powder obtained in the embodiment of the present application can improve the mechanical properties of the aluminum-based composite material obtained based on the powder, and obtain a high-strength, high-toughness and high-rigidity aluminum-based composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of a process for preparing an aluminum-based composite powder according to an embodiment of the present application;
[0032] Figure 2This is a scanning electron microscope image of the first composite powder involved in the embodiment of the present application;
[0033] Figure 3 This is a scanning electron microscope image of the second composite powder involved in the embodiment of the present application.
[0034] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0036] Hereinafter, the embodiment of the method for recovering lithium from waste lithium iron phosphate batteries of the present application is specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the accompanying drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0037] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0038] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0039] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0040] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0041] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0042] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0043] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and understandable, the technical solution of the present application is further described below in conjunction with the accompanying drawings and embodiments. However, the present application is not limited to the listed embodiments, and should also include any other known changes within the scope of the rights claimed in the present application.
[0044] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present application. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0045] In order to better understand the technical solution of the present application, a detailed description will be given below in conjunction with the accompanying drawings and specific implementation methods.
[0046] In conventional technology, the raw material powder (i.e., aluminum-based composite powder) for preparing aluminum-based composite materials usually adopts the method of mechanical powder mixing to introduce nanoparticles into the aluminum powder system. However, there are many problems with this process, mainly including: First, nanoparticles are easy to agglomerate; since nanoparticles have a high specific surface area and surface energy, agglomeration is very easy to occur. Second, the total amount of nanoparticles added is relatively small; since nanoparticles are easy to agglomerate, the agglomeration problem can only be improved by reducing the amount of nanoparticles added, which in turn will lead to a reduction in the effective amount of nanoparticles added in the aluminum-based composite powder, affecting the performance of the aluminum composite material further prepared. Third, the fluidity of the aluminum-based composite powder is poor; since the nanoparticles agglomerate on the surface of the aluminum powder, the fluidity of the aluminum-based composite powder deteriorates, which in turn affects the spreading of the powder, making it easy to produce more hole defects in the further application of the aluminum-based composite powder, affecting the mechanical properties of the prepared material.
[0047] The present application provides a solution, by mechanically mixing aluminum-based raw materials with ceramic nanoparticles accounting for part of the total target addition amount, a first composite powder is obtained; since the single addition amount of ceramic nanoparticles only accounts for a part of the total addition amount, a large number of ceramic nanoparticles can be effectively prevented from agglomerating on the surface of the aluminum alloy powder or forming a pile on the surface of the aluminum alloy powder. Then, the first composite powder is subjected to plasma spheroidization treatment, and with the help of the high temperature of the plasma, the ceramic nanoparticles on the surface of the aluminum-based raw material quickly absorb heat and melt, thereby being integrated into the matrix of the aluminum-based raw material; at the same time, the powder is condensed into spherical droplets under the action of surface tension, and these spherical droplets solidify after cooling, thereby obtaining spherical particles with strong fluidity and dense stacking (i.e., the second composite powder). Then the second composite powder is heat treated; due to the extremely short melting and solidification time in the plasma spheroidization treatment, the morphology of the ceramic nanoparticles in the second composite powder is not very stable, and the heat treatment can just change the crystal structure of the material in the powder; the reorganization of this crystal structure helps to eliminate the defects and stress inside the material, thereby improving the overall stability of the material and avoiding its agglomeration with the newly added particles in the next round of plasma spheroidization treatment to obtain the third composite powder. Then the third composite powder is used as the aluminum-based raw material again, and the above-mentioned mechanical powder mixing, plasma spheroidization treatment and heat treatment steps are repeated until the amount of ceramic nanoparticles added reaches its target total amount, thereby obtaining an aluminum-based composite powder. The aluminum-based composite powder prepared by the above-mentioned step-by-step addition of ceramic nanoparticles and repeated mechanical powder mixing, plasma spheroidization treatment and heat treatment steps has a smooth surface and a regular spherical shape, can effectively improve the distribution uniformity of ceramic nanoparticles in the aluminum-based raw material, avoid the problem of agglomeration caused by adding ceramic nanoparticles once, and the problem of difficulty in plasma spheroidization treatment, and increase the amount of ceramic nanoparticles added to the aluminum alloy composite powder. In the further application process of the aluminum-based composite powder, the aluminum-based composite powder prepared in the embodiment of the present application can improve the mechanical properties of the aluminum-based composite material prepared based on the powder, and obtain a high-strength, high-toughness and high-rigidity aluminum-based composite material.
[0048] A first aspect of an embodiment of the present application provides a method for preparing an aluminum-based composite powder, the method comprising the following steps:
[0049] Step S10, mechanically mixing the aluminum-based raw material and a portion of the ceramic nanoparticles to obtain a first composite powder;
[0050] In a feasible embodiment, an aluminum-based raw material and ceramic nanoparticles are provided, wherein, during the first mechanical mixing, the aluminum-based raw material can be an aluminum alloy powder; the aluminum alloy powder and the ceramic nanoparticles are mechanically mixed to achieve uniform dispersion of the aluminum alloy powder and the ceramic nanoparticles to obtain a first composite powder; wherein the single addition amount of the ceramic nanoparticles during the mechanical mixing accounts for a portion of the total addition amount (i.e., the target total addition amount).
[0051] Mechanical powder mixing is the process of mixing different types of powder materials uniformly by mechanical means. This process usually involves putting multiple powders into mixing equipment, such as ball mills, ultrasonic vibration mixers, air flow mixers, etc., and then using mechanical forces (such as stirring, impact, friction, etc.) to achieve uniform dispersion of powder particles.
[0052] In a feasible embodiment, the target total amount of ceramic nanoparticles added is 2 to 8 wt.%; for example, the target total amount of ceramic nanoparticles added is 2 wt.%, 2.5 wt.%, 3 wt.%, 3.5 wt.%, 4 wt.%, 4.5 wt.%, 5 wt.%, 5.5 wt.%, 6 wt.%, 6.5 wt.%, 7 wt.%, 7.5 wt.%, 8 wt.%, etc. The addition of ceramic nanoparticles can improve the comprehensive performance of the composite material, but if the total amount of ceramic nanoparticles added is too large, the continuity of the aluminum alloy matrix may be gradually destroyed, making the aluminum alloy matrix prone to severe stress concentration during plastic deformation, thereby affecting the overall mechanical properties of the composite material; in addition, the interface wettability between the ceramic nanoparticles and the aluminum matrix may be poor; when the content of ceramic nanoparticles is too high, the interface reaction may be more intense and produce harmful interface products. If the total amount of ceramic nanoparticles added is too small, the advantages of the ceramic nanoparticles may not be fully utilized, and the reinforcing effect on the composite material is limited. Therefore, the target total amount of ceramic nanoparticles added in the present embodiment is determined to be 2-8 wt.%.
[0053] In a feasible embodiment, the single addition amount of ceramic nanoparticles is less than 2wt.%; for example, the single addition amount of ceramic nanoparticles is 1wt.%, 1.1wt.%, 1.2wt.%, 1.3wt.%, 1.4wt.%, 1.5wt.%, 1.6wt.%, 1.7wt.%, 1.8wt.%, 1.9wt.%, etc. If the single addition amount of ceramic nanoparticles is too large, the ceramic nanoparticles will agglomerate on the surface of the aluminum alloy, or form a pile, which will become a defect in the later application process of the aluminum alloy composite powder (i.e., the aluminum alloy composite material), reduce the toughness of the material, and also cause the fluidity of the composite powder to decrease, resulting in the failure of the subsequent plasma spheroidization treatment. If the addition amount is too large, it will lead to an increase in process steps and an increase in production costs.
[0054] Exemplarily, the single addition amount of the ceramic nanoparticles is less than 2 wt.%, and greater than or equal to 1 wt.%.
[0055] For example, in the preparation process of aluminum-based composite powder, the single addition amount of ceramic nanoparticles can be the same or different. For example, the target total addition amount of ceramic nanoparticles is 8wt.%, and the single addition amount of ceramic nanoparticles can be: 1wt.%, 1.5wt.%, 1wt.%, 1.5wt.%, 1.8wt.%, 1.2wt.%.
[0056] In a feasible implementation manner, the aluminum alloy powder includes, by mass percentage, 2-6% Mn, 0.5-1% Sc, and the remainder Al.
[0057] Exemplarily, the aluminum alloy powder includes, by mass percentage, 2-6% Mn, 0.5-1% Sc, and the remainder Al and unavoidable impurity elements.
[0058] Exemplarily, the impurity elements include O, N and H, wherein the O content is less than or equal to 0.08 wt.%, the N content is less than or equal to 0.01 wt.%, and the H content is less than or equal to 0.002 wt.%.
[0059] Exemplarily, the aluminum alloy powder includes: 2-6% Mn, 0.1-5% Mg, 0.5-1% Sc, 0.1-0.5% Zr, and the remainder is Al.
[0060] Exemplarily, the aluminum alloy powder includes: Mn, the content of which can be: 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, etc.; Mg, the content of which can be: 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.; Sc, the content of which can be: 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc.; Zr, the content of which can be: 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, etc. By adding Mn, Mg, Sc, Zr and Al in specific proportions, the aluminum alloy can have excellent properties such as increased strength, enhanced corrosion resistance, refined grains, improved processing performance, increased heat resistance and reduced costs. The improvement of these properties makes aluminum alloy have wider application prospects in aerospace, automobile manufacturing, building materials and electronic products.
[0061] In one possible embodiment, the ceramic nanoparticles include at least one of TiN, TiC, SiC and TiB2.
[0062] TiN is a high-hardness, wear-resistant coating material. Adding it to aluminum alloy can significantly improve the wear resistance and corrosion resistance of aluminum alloy and extend the service life of aluminum alloy.
[0063] TiC can refine the grains of aluminum alloys and is mainly distributed inside the grains, reducing the amount of second phases at the grain boundaries, thereby reducing the intergranular corrosion rate and improving the corrosion resistance of the aluminum alloy. At the same time, TiC particles can also play a role of dispersion strengthening in aluminum alloys, hindering dislocation movement and grain boundary sliding, thereby significantly improving the yield strength and tensile strength of the aluminum alloy.
[0064] The addition of SiC can increase the elastic modulus of aluminum alloy, making it more resistant to deformation; and SiC particles themselves have high hardness and wear resistance, therefore, they can enhance the wear resistance of aluminum-based composite materials and make them have good stability at high temperatures.
[0065] TiB2 plays a role of dispersion strengthening in aluminum alloys, which can significantly improve the strength of aluminum alloys. In specific cases, such as introducing TiB2 into 3D printed aluminum alloys, it can greatly reduce the printing defects of the material and successfully prepare aluminum alloys with ultra-high fatigue strength.
[0066] In one feasible implementation, the particle size of the aluminum alloy powder is 15 to 53 μm; for example, the particle size of the aluminum alloy powder is 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 51 μm, 52 μm, 53 μm, etc. The powder within this range can be adapted to the laser spot diameter, powder layer thickness, laser power, etc. in the process of being applied to the selective laser melting additive manufacturing process, and is more suitable for this process. Therefore, the particle size of the aluminum alloy powder is determined to be 15 to 53 μm.
[0067] In one feasible embodiment, the particle size of the ceramic nanoparticles is 10 to 50 nm; for example, the particle size of the ceramic nanoparticles is 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, etc. If the particle size of the ceramic nanoparticles is too large, it may cause uneven distribution of the ceramic nanoparticles in the aluminum matrix, resulting in reduced connectivity of the matrix and affecting the overall mechanical properties and processing properties of the material obtained after application. In addition, ceramic particles with too large a particle size may introduce more holes and defects in the composite material, which will become stress concentration points in the material and reduce the strength and toughness of the material. If the particle size of the ceramic nanoparticles is too small, it may have a problem of uneven dispersion in the composite material, and agglomerate into larger particles or form precipitates, thereby losing its nano effect and reducing the performance of the material. Therefore, the particle size of the ceramic nanoparticles is determined to be 10 to 50 nm.
[0068] In one feasible implementation, mechanical powder mixing includes: ultrasonic vibration powder mixing. Ultrasonic vibration powder mixing technology uses the high-frequency vibration energy of ultrasound to transmit ultrasound to the powder in the mixing container through a vibrating probe or a vibrating plate. The vibration of ultrasound can break the Coulomb force and electrostatic force between powder particles, causing the powder particles to change from an agglomerated state to a dispersed state, thereby making it easier to achieve uniform mixing.
[0069] In a feasible implementation manner, the powder mixing time of the ultrasonic vibration powder mixing is 10 to 30 minutes; for example, the powder mixing time is 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, etc.
[0070] Exemplarily, the temperature of the ultrasonic vibration powder mixing may be room temperature, and the ultrasonic power may be 50-200W.
[0071] Step S20, performing plasma spheroidization treatment on the first composite powder to obtain a second composite powder;
[0072] In one feasible embodiment, the first composite powder is subjected to plasma spheroidization treatment, and the high temperature of the plasma is used to cause the ceramic nanoparticles on the surface of the aluminum-based raw material to quickly absorb heat and melt, thereby being integrated into the matrix of the aluminum-based raw material; at the same time, the powder is condensed into spherical droplets under the action of surface tension, and these spherical droplets solidify after cooling, thereby obtaining spherical particles with strong fluidity and dense packing (i.e., the second composite powder).
[0073] It should be understood that if too many ceramic nanoparticles are added at one time during mechanical powder mixing, the ceramic nanoparticles are likely to agglomerate on the surface of the aluminum-based raw material, causing the fluidity of the composite powder to drop sharply and leading to the failure of the plasma spheroidization treatment.
[0074] In one feasible embodiment, the powder feeding rate of the plasma spheroidization treatment is 30 to 100 g / min; for example, the powder feeding rate of the plasma spheroidization treatment is 30 g / min, 40 g / min, 50 g / min, 60 g / min, 70 g / min, 80 g / min, 90 g / min, 100 g / min, etc. When the powder feeding rate is too low, the unit mass of powder stays in the plasma for a relatively long time, absorbing too much heat, which may cause the powder to gasify. This not only reduces the yield of spherical powder, but also may adsorb a large amount of small particles of powder on the surface of the particles, affecting the purity and sphericity of the powder. At the same time, due to powder gasification and small particle adsorption, the actual yield of spherical powder will be significantly reduced, increasing production costs and the difficulty of waste treatment. When the powder feeding rate is too high, the heat absorbed by the unit mass of powder in the plasma is not enough to melt all powder particles. This will cause some powder particles to fail to melt completely, forming defects such as satellite balls and coated powder, and reducing the spheroidization rate of the powder; and excessive powder feeding rate may also cause the plasma torch to form a large temperature gradient, or even cause the plasma torch to go out. This will seriously affect the stability and efficiency of the spheroidization process. Therefore, the embodiment of the present application determines that the powder feeding rate of the ion spheroidization treatment is 30 to 100 g / min. At this rate, the powder particles can be fully melted in the plasma and condensed into spherical powder under the action of surface tension and high temperature gradient. At the same time, this rate should also ensure the stability and efficiency of the plasma torch to reduce unnecessary energy loss and production costs.
[0075] In one feasible embodiment, the reaction chamber pressure of the plasma spheroidization treatment is 13 to 18 psi; for example, the reaction chamber pressure of the plasma spheroidization treatment is 13 psi, 13.5 psi, 14 psi, 14.5 psi, 15 psi, 15.5 psi, 16 psi, etc. When the reaction chamber pressure is too high, it may cause plasma instability, affecting the uniformity and efficiency of the spheroidization process; and in order to maintain a higher pressure, more energy is consumed, increasing production costs; in addition, long-term operation under high pressure may cause wear and tear on the equipment and shorten its service life. When the reaction chamber pressure is too low, the powder may stay in the plasma for too short a time and cannot be fully melted and spheroidized; and the plasma density under low pressure may not be sufficient to provide sufficient energy to melt the powder particles. Therefore, the embodiment of the present application determines that the reaction chamber pressure of the plasma spheroidization treatment is 13 to 18 psi.
[0076] In one feasible embodiment, the power of the plasma spheroidization treatment is 30 to 50 KW; for example, the power of the plasma spheroidization treatment is 30 KW, 32 KW, 34 KW, 36 KW, 38 KW, 40 KW, 42 KW, 44 KW, 46 KW, 48 KW, 50 KW, etc. When the power is too large, the powder particles may overheat or even gasify, reducing the yield of the spherical powder, and high-power operation will consume more electricity and increase production costs. When the power is too small, the powder particles may not be fully melted, forming incomplete spherical powders, and the spheroidization process under low power may be relatively slow, reducing production efficiency. Therefore, the embodiment of the present application determines that the power of the plasma spheroidization treatment is 30 to 50 KW.
[0077] In one feasible embodiment, the flow rate of the central gas argon gas in the plasma spheroidization treatment is 15 to 25 slpm; for example, the central gas argon gas in the plasma spheroidization treatment is 15 slpm, 16 slpm, 17 slpm, 18 slpm, 19 slpm, 20 slpm, 21 slpm, 22 slpm, 23 slpm, 24 slpm, 25 slpm, etc. Too much central gas argon gas may limit the diffusion range of the plasma, affect the uniformity of the spheroidization process, and in order to maintain a higher gas flow rate, more energy needs to be consumed. When the central gas argon gas is too small, it may cause the plasma stability to decrease, affecting the spheroidization effect. At the same time, insufficient gas flow may not provide sufficient protective atmosphere for the powder particles, resulting in unsatisfactory spheroidization effect. Therefore, the embodiment of the present application determines that the flow rate of the central gas argon gas in the plasma spheroidization treatment is 15 to 25 slpm.
[0078] In one feasible embodiment, the flow rate of the sheath gas argon for the plasma spheroidization treatment is 45 to 60 slpm; for example, the sheath gas argon for the plasma spheroidization treatment is 45 slpm, 46 slpm, 48 slpm, 50 slpm, 52 slpm, 54 slpm, 56 slpm, 58 slpm, 60 slpm, etc. Too much sheath gas argon may dilute the plasma, reduce its energy density and temperature, and too large a sheath gas flow rate may interfere with the movement trajectory and melting process of the powder particles in the plasma. Too little sheath gas argon may not provide enough protective atmosphere for the plasma, resulting in contamination or instability of the plasma, and the powder particles may face oxidation risks. Therefore, the embodiment of the present application determines that the flow rate of the sheath gas argon for plasma spheroidization treatment is 45 to 60 slpm.
[0079] In one feasible implementation, the flow rate of the carrier gas for the plasma spheroidization treatment is 2 to 5 slpm; for example, the carrier gas for the plasma spheroidization treatment is 2 slpm, 2.5 slpm, 3 slpm, 3.5 slpm, 4 slpm, 4.5 slpm, 5 slpm, etc. Excessive carrier gas flow rate may cause uneven dispersion of powder particles in the reaction chamber, affecting the spheroidization effect, and more energy is required to maintain a higher gas flow rate. However, a carrier gas flow rate that is too small may not be able to effectively transport powder particles into the reaction chamber, resulting in the inability to carry out the spheroidization process. At the same time, insufficient carrier gas flow rate will limit the conveying speed of the powder, thereby reducing production efficiency. Therefore, the embodiment of the present application determines that the flow rate of the carrier gas for plasma spheroidization treatment is 2 to 5 slpm.
[0080] Exemplarily, the plasma spheroidization process parameters are: power 40KW, powder feeding rate 38g / min, center gas argon 19.5slpm, sheath gas argon 55slpm, carrier gas 3.5slpm, reaction chamber pressure 14.7psi.
[0081] For example, refer to Figure 2 , is a scanning electron microscope image of the first composite powder obtained by mechanically mixing the aluminum-based raw material and a portion of the ceramic nanoparticles; Figure 2 It can be seen that by reducing the single addition amount of ceramic nanoparticles, the ceramic nanoparticles can just cover the surface of the aluminum-based raw material after mechanical powder mixing, avoiding the occurrence of agglomeration. Figure 3 , is a scanning electron microscope image of a second composite powder obtained after the first composite powder is subjected to plasma spheroidization treatment; Figure 3 It can be seen that through further plasma spheroidization treatment, with the help of the high temperature of plasma, the ceramic nanoparticles on the surface of the aluminum-based raw material quickly absorb heat and melt, and then integrate into the matrix of the aluminum-based raw material; at the same time, under the action of surface tension, the powder is condensed into spherical droplets, and these spherical droplets solidify after cooling, thus obtaining spherical particles with strong fluidity and dense packing.
[0082] Step S30, heat treating the second composite powder to obtain a third composite powder;
[0083] In a feasible embodiment, due to the extremely short melting and solidification time in the plasma spheroidization treatment, the morphology of the ceramic nanoparticles in the second composite powder is not very stable, and heat treatment can just change the crystal structure of the material in the powder; the reorganization of this crystal structure helps to eliminate defects and stresses inside the material, thereby improving the overall stability of the material and preventing it from agglomerating with newly added particles in the next round of plasma spheroidization treatment; therefore, the second composite powder is heat treated to obtain a third composite powder.
[0084] In one feasible embodiment, the temperature of the heat treatment is 400-500°C; for example, the temperature of the heat treatment is 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, etc. When the heat treatment temperature is too high, the grains of the powder will grow rapidly, resulting in excessive or irregular grain size. This will reduce the hardness and toughness of the material, while reducing its strength and durability. At the same time, excessively high temperatures may also cause local melting of the material, making the organizational structure unstable, further affecting the performance of the material. When the heat treatment temperature is too low, the stress inside the material may not be fully released, resulting in poor improvement in the stability of the mixed powder. Therefore, the embodiment of the present application determines that the temperature of the heat treatment is 400-500°C.
[0085] In one feasible implementation, the holding time of the heat treatment is 2 to 6 hours; for example, the holding time is 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, etc. Too long a heat treatment time will cause uneven grain growth inside the material, thereby affecting the overall performance and quality of the material; and in some cases, too long a heat treatment time will also increase the risk of surface oxidation and decarburization of the material, further reducing the performance of the material, while consuming more energy and increasing production costs. A short holding time may result in an uneven internal organizational structure of the material, resulting in a poor improvement in the stability of the mixed powder. Therefore, the embodiment of the present application determines that the holding time of the heat treatment is 2 to 6 hours.
[0086] Step S40, when the current total amount of the ceramic nanoparticles added is less than the target total amount, the third composite powder is used as the aluminum-based raw material, and the step of mechanically mixing the aluminum-based raw material and part of the ceramic nanoparticles is returned to be executed until the current total amount of the ceramic nanoparticles added is equal to the target total amount, and the third composite powder is determined as the aluminum-based composite powder.
[0087] In a feasible embodiment, when the third composite powder is obtained, it is determined whether the current total amount of ceramic nanoparticles added is less than the target total amount of ceramic nanoparticles added; when the current total amount of ceramic nanoparticles added is less than the target total amount of ceramic nanoparticles added, the third composite powder is used as the aluminum-based raw material again, and mechanically mixed with at least part of the remaining ceramic nanoparticles again, and subsequent steps are performed; until the current total amount of ceramic nanoparticles added is equal to the target total amount of ceramic nanoparticles added, the obtained third composite powder is an aluminum-based composite powder.
[0088] In this embodiment, the first composite powder is obtained by mechanically mixing the aluminum-based raw material with the ceramic nanoparticles accounting for part of the total amount of the target addition; since the single addition amount of the ceramic nanoparticles only accounts for a part of the total amount of the addition, it is possible to effectively avoid a large number of ceramic nanoparticles from agglomerating on the surface of the aluminum alloy powder or forming a pile on the surface of the aluminum alloy powder. Then, the first composite powder is subjected to plasma spheroidization treatment, and the ceramic nanoparticles on the surface of the aluminum-based raw material absorb heat and melt rapidly by means of the high temperature of the plasma, thereby being integrated into the matrix of the aluminum-based raw material; at the same time, the powder is condensed into spherical droplets under the action of surface tension, and these spherical droplets solidify after cooling, thereby obtaining spherical particles (i.e., the second composite powder) with strong fluidity and compact stacking. Then the second composite powder is heat treated; due to the extremely short melting and solidification time in the plasma spheroidization treatment, the morphology of the ceramic nanoparticles in the second composite powder is not very stable, and the heat treatment can just change the crystal structure of the material in the powder; the reorganization of this crystal structure helps to eliminate the defects and stress inside the material, thereby improving the overall stability of the material and avoiding its agglomeration with the newly added particles in the next round of plasma spheroidization treatment to obtain the third composite powder. Then the third composite powder is used as the aluminum-based raw material again, and the above-mentioned mechanical powder mixing, plasma spheroidization treatment and heat treatment steps are repeated until the amount of ceramic nanoparticles added reaches its target total amount, thereby obtaining an aluminum-based composite powder. The aluminum-based composite powder prepared by the above-mentioned step-by-step addition of ceramic nanoparticles and repeated mechanical powder mixing, plasma spheroidization treatment and heat treatment steps has a smooth surface and a regular spherical shape, can effectively improve the distribution uniformity of ceramic nanoparticles in the aluminum-based raw material, avoid the problem of agglomeration caused by adding ceramic nanoparticles once, and the problem of difficulty in plasma spheroidization treatment, and increase the amount of ceramic nanoparticles added to the aluminum alloy composite powder. In the further application process of the aluminum-based composite powder, the aluminum-based composite powder prepared in the embodiment of the present application can improve the mechanical properties of the aluminum-based composite material prepared based on the powder, and obtain a high-strength, high-toughness and high-rigidity aluminum-based composite material.
[0089] Furthermore, the present invention also provides a method for preparing an aluminum-based composite material, which comprises the following steps:
[0090] Step A10, providing an aluminum-based composite powder, wherein the aluminum-based composite powder is prepared by the above method;
[0091] In a feasible embodiment, an aluminum-based raw material and a portion of ceramic nanoparticles are mechanically mixed to obtain a first composite powder, wherein the aluminum-based raw material includes: aluminum alloy powder; the first composite powder is plasma spheroidized to obtain a second composite powder; the second composite powder is heat treated to obtain a third composite powder; when the current total amount of the ceramic nanoparticles added is less than the target total amount, the third composite powder is used as the aluminum-based raw material, and the step of mechanically mixing the aluminum-based raw material and a portion of the ceramic nanoparticles is returned to execute until the current total amount of the ceramic nanoparticles added is equal to the target total amount, and the third composite powder is determined as the aluminum-based composite powder.
[0092] Exemplarily, the target total amount of the ceramic nanoparticles added is 2-8 wt.%, and the single amount of the ceramic nanoparticles added is less than 2 wt.%.
[0093] Exemplarily, the aluminum alloy powder includes, by mass percentage: 2-6% Mn, 0.5-1% Sc, and the remainder Al;
[0094] And / or, the ceramic nanoparticles include at least one of TiN, TiC, SiC and TiB2.
[0095] Exemplarily, the particle size of the aluminum alloy powder is 15 to 53 μm;
[0096] And / or the particle size of the ceramic nanoparticles is 10 to 50 nm.
[0097] Exemplarily, the mechanical powder mixing includes: ultrasonic vibration powder mixing, and the powder mixing time is 10 to 30 minutes.
[0098] Exemplarily, the powder feeding rate of the plasma spheroidization treatment is 30 to 100 g / min;
[0099] and / or, the reaction chamber pressure of the plasma spheroidization treatment is 13 to 18 psi;
[0100] And / or, the power of the plasma spheroidization treatment is 30 to 50 KW;
[0101] and / or, the central gas argon gas of the plasma spheroidization treatment is 15 to 25 slpm;
[0102] and / or, the sheath gas argon gas of the plasma spheroidization treatment is 45 to 60 slpm;
[0103] And / or, the carrier gas for the plasma spheroidization treatment is 2 to 5 slpm.
[0104] Exemplarily, the heat treatment temperature is 400-500° C., and the holding time is 2-6 hours.
[0105] Step A20, performing selective laser melting treatment on the aluminum-based composite powder to obtain an aluminum-based composite material.
[0106] In a feasible embodiment, the aluminum-based composite powder is subjected to selective laser melting treatment to obtain an aluminum-based composite material; and the obtained aluminum-based composite material has the characteristics of high strength, high toughness and high stiffness, with a strength ≥650MPa, an elongation ≥5%, and an elastic modulus between 75-95GPa (varies with the content of ceramic nanoparticles), which is significantly better than the aluminum-based composite material prepared using aluminum-based composite powder obtained by mechanical powder mixing alone as raw material.
[0107] Exemplarily, the laser power of the selective laser melting process may be 100-300 W; for example, 100 W, 150 W, 200 W, 250 W, 300 W, etc.
[0108] Exemplarily, the scanning speed of the selective laser melting process can be 900-1200 mm / s; for example, 900 mm / s, 950 mm / s, 1050 mm / s, 1100 mm / s, 1150 mm / s, 1200 mm / s, etc.
[0109] Exemplarily, the thickness of the powder layer processed by the selective laser melting process may be 30 to 40 μm; for example, 30 μm, 32 μm, 34 μm, 36 μm, 38 μm, 40 μm, etc.
[0110] Exemplarily, the scanning pitch of the selective laser melting process can be 80 to 120 μm; for example, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm, 105 μm, 110 μm, 115 μm, 120 μm, etc.
[0111] Exemplarily, the aluminum-based composite powder is subjected to selective laser melting treatment to obtain a laser prefabricated aluminum matrix; the laser prefabricated aluminum matrix is subjected to heat treatment to obtain an aluminum-based composite material, wherein the heat treatment temperature is 300-400°C (for example, 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, etc.), and the heat preservation time is 3-6h (for example, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, etc.). Heat treatment can strengthen the aluminum-based composite material, improve the interface bonding strength, regulate the mechanical properties, and affect the damping performance, so as to optimize the organizational structure and performance of the composite material and meet different application requirements.
[0112] In this embodiment, the raw material used for the aluminum-based composite material is prepared by adding ceramic nanoparticles in steps and repeatedly performing the steps of mechanical powder mixing, plasma spheroidization treatment and heat treatment; and the above process can effectively improve the distribution uniformity of ceramic nanoparticles in the aluminum-based raw material, avoid the problem of agglomeration caused by adding ceramic nanoparticles at one time, and the occurrence of difficulties in plasma spheroidization treatment, and increase the amount of ceramic nanoparticles added to the aluminum alloy composite powder; therefore, the aluminum-based composite material further prepared based on the aluminum-based composite powder has the characteristics of high strength, high toughness and high stiffness.
[0113] In order to enable the details and operations of the above embodiments of the present application to be clearly understood by those skilled in the art, and to significantly demonstrate the improved performance of the embodiments of the present application, the above technical solutions are illustrated by means of multiple embodiments below.
[0114] Example 1
[0115] (1) mixing 41 μm Al-Mn-Sc alloy powder and 25 nm TiN by ultrasonic vibration for 40 minutes to obtain a first composite powder, wherein the Al-Mn-Sc alloy powder has the following components: Mn 3 wt.%, Sc 0.7 wt.%, and the balance Al;
[0116] (2) performing plasma spheroidization treatment on the first composite powder to obtain a second composite powder, wherein the plasma spheroidization treatment process parameters are: power 40KW, powder feeding rate 38g / min, center gas argon 19.5slpm, sheath gas argon 55slpm, carrier gas 3.5slpm, reaction chamber pressure 14.7psi;
[0117] (3) heat treating the second composite powder to obtain a third composite powder, wherein the heat treatment temperature is 450° C. and the holding time is 3 h;
[0118] (4) mixing the third composite powder with 25 nm TiN by ultrasonic vibration for 40 minutes, and performing steps (2) and (3) until the total amount of TiN added is 2 wt.%, to obtain an aluminum-based composite powder, wherein the TiN is added to the aluminum-based raw material in two times, and the single addition amount of TiN is 1 wt.% and 1 wt.% respectively;
[0119] (5) The aluminum-based composite powder is subjected to selective laser melting and heat treatment at 300° C. for 4 h to obtain an aluminum-based composite material, wherein the process parameters of the selective laser melting treatment are: laser power 200 W, scanning speed 1000 mm / s, powder layer thickness 36 μm, and scanning spacing 110 μm.
[0120] Example 2
[0121] (1) mixing 25 μm Al-Mn-Sc alloy powder and 15 nm TiN by ultrasonic vibration for 40 minutes to obtain a first composite powder, wherein the Al-Mn-Sc alloy powder has the following components: Mn 3 wt.%, Sc 0.7 wt.%, and the balance Al;
[0122] (2) performing plasma spheroidization treatment on the first composite powder to obtain a second composite powder, wherein the plasma spheroidization treatment process parameters are: power 40KW, powder feeding rate 38g / min, center gas argon 19.5slpm, sheath gas argon 55slpm, carrier gas 3.5slpm, reaction chamber pressure 14.7psi;
[0123] (3) heat treating the second composite powder to obtain a third composite powder, wherein the heat treatment temperature is 450° C. and the holding time is 3 h;
[0124] (4) mixing the third composite powder with 15 nm TiN by ultrasonic vibration for 40 minutes, and performing steps (2) and (3) until the total amount of TiN added is 5 wt.%, to obtain an aluminum-based composite powder, wherein TiN is added to the aluminum-based raw material in 4 times, and the single addition amount of TiN is 1.5 wt.%, 1 wt.%, 1.5 wt.% and 1 wt.% respectively;
[0125] (5) The aluminum-based composite powder is subjected to selective laser melting and heat treatment at 300° C. for 4 h to obtain an aluminum-based composite material, wherein the process parameters of the selective laser melting treatment are: laser power 200 W, scanning speed 1000 mm / s, powder layer thickness 36 μm, and scanning spacing 110 μm.
[0126] Example 3
[0127] (1) 38 μm Al-Mn-Sc alloy powder and 20 nm TiN are subjected to ultrasonic vibration mixing for 40 minutes to obtain a first composite powder, wherein the Al-Mn-Sc alloy powder has the following components: Mn 3 wt.%, Sc 0.7 wt.%, and the balance Al;
[0128] (2) performing plasma spheroidization treatment on the first composite powder to obtain a second composite powder, wherein the plasma spheroidization treatment process parameters are: power 40KW, powder feeding rate 38g / min, center gas argon 19.5slpm, sheath gas argon 55slpm, carrier gas 3.5slpm, reaction chamber pressure 14.7psi;
[0129] (3) heat treating the second composite powder to obtain a third composite powder, wherein the heat treatment temperature is 450° C. and the holding time is 3 h;
[0130] (4) the third composite powder is mixed with 20 nm TiN by ultrasonic vibration for 40 minutes, and steps (2) and (3) are performed until the total amount of TiN added is 8 wt.%, to obtain an aluminum-based composite powder, wherein TiN is added to the aluminum-based raw material in 4 times, and the single addition amount of TiN is 2 wt.%;
[0131] (5) The aluminum-based composite powder is subjected to selective laser melting and heat treatment at 300° C. for 4 h to obtain an aluminum-based composite material, wherein the process parameters of the selective laser melting treatment are: laser power 200 W, scanning speed 1000 mm / s, powder layer thickness 36 μm, and scanning spacing 110 μm.
[0132] Comparative Example 1
[0133] The experimental steps are the same as those of Example 3, except that 2 wt. % of TiN is added into the Al-Mn-Sc alloy powder at one time and then ultrasonically vibrated and mixed.
[0134] Comparative Example 2
[0135] The experimental steps are the same as those of Example 2, except that 5 wt. % of TiN is added into the Al-Mn-Sc alloy powder at one time and then ultrasonically vibrated and mixed.
[0136] Comparative Example 3
[0137] The experimental steps are the same as those of Example 1, except that 8 wt. % of TiN is added into the Al-Mn-Sc alloy powder at one time and then ultrasonically vibrated and mixed.
[0138] Comparative Example 4
[0139] The experimental steps are the same as those of Example 2, except that step (3) of heat treating the powder is no longer performed, that is, only the process steps of combining ultrasonic vibration powder mixing with plasma spherical treatment are performed multiple times.
[0140] Comparative Example 5
[0141] The experimental steps are the same as those of Example 2, except that the order of steps (2) and (3) is reversed, that is, after the first composite powder is obtained by ultrasonic vibration mixing, the first composite powder is first heat treated, and then the heat treated composite powder is plasma treated.
[0142] The mechanical properties of the aluminum-based composite materials of Comparative Examples 1 to 5 and Examples 1 to 3 were tested, and the experimental results are shown in Table 1 below:
[0143] Table 1
[0144]
[0145] According to the mechanical property test results of the above-mentioned Examples 1 to 3, it can be seen that with the increase in the amount of ceramic nanoparticles added, the yield strength, tensile strength and elastic modulus of the obtained aluminum-based composite material increase, especially the elastic modulus increases significantly; although the elongation decreases, it still remains at a relatively high level of >5% (higher than comparative examples 1 to 5).
[0146] According to the mechanical property test results of the above-mentioned comparative examples 1 to 3, it can be seen that with the increase in the amount of ceramic nanoparticles added, the elongation of the obtained aluminum-based composite material is significantly reduced; this may be because with the addition of ceramic nanoparticles, the ceramic nanoparticles agglomerate and become weak points and defects inside the material, which in turn leads to a decrease in elongation, while the enhancement effects of yield strength, tensile strength and elastic modulus are poor, among which the yield strength and tensile strength are maintained in the range of 580 to 600 MPa, and the elastic modulus is improved, but the improvement effect is worse than that of Examples 1 to 3, which may be due to the agglomeration of ceramic nanoparticles, resulting in a reduction in the effective amount of ceramic nanoparticles added.
[0147] According to the above-mentioned Example 2 and Comparative Example 4, since the second composite powder is not heat treated, it is difficult to further homogenize the distribution of ceramic nanoparticles in the second composite powder after plasma spheroidization, so that there is still a certain degree of agglomeration of ceramic nanoparticles inside the powder, which causes the elongation of the aluminum-based composite material to be still low.
[0148] According to the above-mentioned Example 2 and Comparative Example 5, after the order of heat treatment and plasma treatment is swapped, the first heat treatment is equivalent to heat treatment of the alloy powder, which has no effect on improving the uniformity of the composite powder after spheroidization, and thus the elongation is also maintained at a low level.
[0149] The above are only preferred embodiments of the present application, and do not limit the scope of the present application. For those skilled in the art, the present application may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of patent protection of the present application.
Claims
1. A method for preparing aluminum-based composite powder, characterized in that: The method for preparing the aluminum-based composite powder comprises the following steps: Mechanically mixing the aluminum-based raw material and a portion of the ceramic nanoparticles to obtain a first composite powder; performing plasma spheroidization treatment on the first composite powder to obtain a second composite powder; heat treating the second composite powder to obtain a third composite powder; In the case where the current total amount of the ceramic nanoparticles added is less than the target total amount, the third composite powder is used as the aluminum-based raw material, and the step of mechanically mixing the aluminum-based raw material and part of the ceramic nanoparticles is returned to be executed until the current total amount of the ceramic nanoparticles added is equal to the target total amount, and the third composite powder is determined as an aluminum-based composite powder, wherein the target total amount of the ceramic nanoparticles added is 2 to 8 wt.%, and the single amount of the ceramic nanoparticles added is less than 2 wt.%.
2. The method for preparing aluminum-based composite powder according to claim 1, characterized in that: The ceramic nanoparticles include at least one of TiN, TiC, SiC and TiB2.
3. The method for preparing aluminum-based composite powder according to claim 1, characterized in that: The aluminum-based raw material that is initially mechanically mixed with the ceramic nanoparticles is selected from aluminum alloy powder; In terms of mass percentage, the aluminum alloy powder comprises: 2-6% Mn, 0.5-1% Sc, and the remainder Al; or, In terms of mass percentage, the aluminum alloy powder includes: 2-6% Mn, 0.1-5% Mg, 0.5-1% Sc, 0.1-0.5% Zr, and the rest is Al.
4. The method for preparing aluminum-based composite powder according to claim 1, characterized in that: The particle size of the aluminum alloy powder is 15 to 53 μm; And / or, the particle size of the ceramic nanoparticles is 10 to 50 nm.
5. The method for preparing aluminum-based composite powder according to claim 1, characterized in that: The mechanical powder mixing includes: ultrasonic vibration powder mixing, and the powder mixing time is 10 to 30 minutes.
6. The method for preparing aluminum-based composite powder according to claim 1, characterized in that: The powder feeding rate of the plasma spheroidization treatment is 30 to 100 g / min; and / or, the reaction chamber pressure of the plasma spheroidization treatment is 13 to 18 psi; And / or, the power of the plasma spheroidization treatment is 30 to 50 KW; and / or, the flow rate of the central gas argon gas in the plasma spheroidization treatment is 15 to 25 slpm; and / or, the flow rate of the sheath gas argon gas in the plasma spheroidization treatment is 45 to 60 slpm; And / or, the flow rate of the carrier gas in the plasma spheroidization treatment is 2 to 5 slpm.
7. The method for preparing aluminum-based composite powder according to claim 1, characterized in that: The heat treatment temperature is 400-500° C., and the heat preservation time is 2-6 hours.
8. An aluminum-based composite powder, characterized in that: The aluminum-based composite powder is prepared by the method according to any one of claims 1 to 7.
9. A method for preparing an aluminum-based composite material, characterized in that: The method for preparing the aluminum-based composite material comprises the following steps: Providing an aluminum-based composite powder, wherein the aluminum-based composite powder is prepared by the method according to any one of claims 1 to 7; The aluminum-based composite powder is subjected to selective laser melting treatment to obtain an aluminum-based composite material.
10. An aluminum-based composite material, characterized in that: The aluminum-based composite material comprises an aluminum-based composite powder prepared by the method according to any one of claims 1 to 7, or is prepared by the method for preparing an aluminum-based composite material according to claim 9.
Citation Information
Patent Citations
Nano ceramic reinforced high-entropy alloy composite powder for additive manufacturing as well as preparation method and application thereof
CN111168057A
Nano ceramic metal composite powder for 3D printing and application
CN111940723A
Method for preparing multi-scale ceramic phase reinforced metal composite material by 3D printing
CN111957967A
Laser cladding ceramic particle reinforced aluminum-based cladding layer and preparation method thereof
CN115287647A
A method of fabricating an aluminum matrix composite and an aluminum matrix composite fabricated by the same
KR1020160071284A