Hollow drum repairing material in building construction field, preparation method thereof and hollow drum repairing method
By using a combination of specific powders and emulsions in hollow repair materials, the problems of weak adhesion, insufficient flow and long settling time in the prior art are solved, efficient and environmentally friendly hollow repair is achieved, and construction is simplified Process and reduce costs.
Patent Information
- Application Number
- CN202411114071.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The existing hollow restoration materials have weak bonding power, insufficient flow, too long settling time, complex construction technology and unenvironmental protection, resulting in long construction cycles and high costs.
Use quick-setting repair mortar composed of powder and emulsion, which includes silicate cement, sulfoaluminate cement, quartz powder, cellulose ether, tartaric acid, water reducer, defoaming agent and lithium carbonate. The weight ratio of material to emulsion is 1:0.34-0.38, and the material performance and convenience are ensured by the two-component preparation on the construction site.
It achieves the effects of high bond strength, strong fluidity, rapid solidification, waterproofing and cracking, shortens the construction cycle, reduces costs, and improves the quality and safety of repairs.
Smart Images

Figure BDA0004993133950000051 
Figure BDA0004993133950000061 
Figure BDA0004993133950000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to a hollow repair material in the field of building construction, a preparation method thereof and a hollow repair method. Background Art
[0002] In recent years, as ceramic tiles are used more and more widely in buildings, after a long period of time, due to environmental factors such as temperature differences and humidity changes, as well as limitations of the tile bonding process, the tiles may peel off and fall off from the base of the building structure, which not only seriously affects the appearance of the building, but also poses a serious safety hazard.
[0003] In the prior art, once hollow tiles appear, they are usually replaced and re-applied or glue is injected for repair. It is necessary to check whether the wall or floor is hollow or damaged, knock off the damaged part, clean the work surface, re-paste the tiles or repair the wall and floor to make it flat, clean the tiles or base surface after the glue or adhesive material is dry, and use it after it is completely solidified and has strength.
[0004] However, the hollow repair materials currently on the market have the following problems, such as: weak adhesion of the repair materials, insufficient fluidity, too long setting time, complex construction process, and environmentally unfriendly materials. Summary of the invention
[0005] In order to solve the problems existing in the prior art, one of the purposes of the present invention is to provide a hollow repair material in the field of construction. The hollow repair material is a fast-setting repair mortar with the advantages of high bonding strength, strong fluidity, rapid solidification, waterproofness, and anti-cracking. It can not only effectively shorten the construction period, but also effectively reduce costs and reduce renovation costs.
[0006] Another object of the present invention is to provide a method for preparing the hollow repair material. The preparation method is simple and can be prepared and used on site, which can effectively shorten the construction period and reduce costs.
[0007] Another object of the present invention is to provide a hollow repair method, which uses the hollow repair material to perform repair, and has the effects of simple and fast construction and good pasting quality.
[0008] The present invention provides a hollow repair material in the field of building construction, wherein the hollow repair material is composed of powder and emulsion, wherein the weight ratio of the powder to the emulsion is 1:0.34-0.38;
[0009] The powder is composed of the following components in weight percentage: 10-30% of silicate cement, 60-80% of sulphoaluminate cement, 5-15% of quartz powder, 0.02-0.1% of cellulose ether, 0.01-0.1% of tartaric acid, 0.05-0.2% of water reducing agent, 0.01-0.1% of defoaming agent and 0.01-0.1% of lithium carbonate.
[0010] It adopts the form of two components (powder + emulsion) and is mixed on-site when used, which is convenient for ensuring the performance of the hollow repair material while taking into account the convenience of use.
[0011] In the hollow repair material, the weight ratio of powder to emulsion is 1:0.34-0.38. Under the composition and proportion of the powder, the inventor fully considers the characteristics of the components, the synergistic relationship between the components, and multiple experiments to conclude that this ratio has a better effect, which is convenient for preparation and operation, and can ensure the construction effect.
[0012] It should be noted that, in the present invention, the weight percentage of each component of the powder is the percentage of the total weight of the powder, rather than the percentage of the total weight of the hollow repair material.
[0013] Furthermore, the silicate cement is general-purpose silicate cement, and the sulphoaluminate cement is fast-hardening sulphoaluminate cement.
[0014] General purpose Portland cement is a hydraulic cementitious material made of Portland cement clinker, an appropriate amount of gypsum, and specified mixed materials. Silicates in mortar promote the crystallization and bonding between cement particles, thereby improving the strength and stability of the mortar. Silicate additives can also improve the durability of the mortar, resist corrosion and erosion by water, gas and chemicals, thereby increasing the service life of the mortar.
[0015] Rapid-hardening sulphoaluminate cement is a hydraulic cementitious material with high early strength made by grinding the calcined clinker with anhydrous calcium sulphoaluminate and dicalcium silicate as the main mineral components together with a small amount of limestone and an appropriate amount of gypsum. In addition to the functions of the above-mentioned general-purpose silicate cement, rapid-hardening sulphoaluminate cement also has the remarkable characteristic of rapid coagulation; low alkalinity and slightly slow foaming speed, which is conducive to process operation and foam stabilization.
[0016] The hollow repair material contains quartz powder, which is a mineral with high hardness and stability, excellent mechanical strength and chemical stability, and can enhance the wear resistance and corrosion resistance of the mortar, and improve the compressive strength and tensile strength of the mortar. Secondly, quartz powder can improve the rheological properties of the mortar, improve its plasticity and processability, reduce loss and water seepage during the construction process, and thus improve the construction efficiency and quality of the mortar.
[0017] Cellulose ether is added to the hollow repair material, and the cellulose ether can increase the bonding force, improve the ductility, fluidity and crack resistance, and has the functions of water retention and air entrainment.
[0018] Tartaric acid is added to the hollow repair material, and tartaric acid can effectively reduce the foam generation in the cement mixture, make the cement surface smoother, and avoid defects such as pitting and bubbles. Through the defoaming effect of tartaric acid, the surface quality of the slurry can be greatly improved. Tartaric acid also has a certain waterproof effect. It can react with cement in the cement mixture to form a waterproof film to prevent water penetration, improve the water resistance and durability of cement components, ensure the quality and stability of the ground, and reduce cracking and gas. Tartaric acid can improve the fluidity of the slurry, make it smoother during construction, reduce the viscosity and surface tension of cement, promote the flow between cement particles, and make the construction effect more high-quality.
[0019] A water reducing agent is added to the hollow repair material, and the water reducing agent can reduce the amount of water used and improve the compression resistance and tensile resistance of the mortar.
[0020] A defoaming agent is added to the hollow repair material, and the defoaming agent can reduce the generation of bubbles and improve the strength and fluidity.
[0021] Lithium carbonate is added to the hollow repair material, and lithium carbonate can improve the material's crack resistance, strength, fluidity, lubrication construction properties, and delay carbonization.
[0022] Emulsion is added to the hollow repair material, and the emulsion mainly provides adhesion, increases construction performance and fluidity, prevents cracking, and has waterproof performance.
[0023] Furthermore, the water reducing agent is a polycarboxylic acid water reducing agent.
[0024] Furthermore, the defoaming agent is a polyether defoaming agent.
[0025] Furthermore, the emulsion is an acrylic emulsion with a concentration of 10-30wt%
[0026] The present invention also provides a method for preparing a hollow drum repair material, comprising the following steps:
[0027] S1. According to the ratio of the hollow drum repair material, weigh each component for later use;
[0028] S2. Add the emulsion into a container, then add the powder, and stir evenly to obtain the hollow repair material.
[0029] Further, in step S2, the stirring speed is 135-145r / min, the stirring time is 2-3 minutes, and the mixture can be used for construction after being stirred evenly. After standing, stirring again can ensure that the hollow drum repair material is mixed evenly, thereby ensuring the construction quality.
[0030] The present invention also provides a hollow repair method in the field of construction, using the hollow repair material to repair the hollow. Specifically, the hollow repair material is used to repair the hollow of tiles or the hollow of wall and floor mortar.
[0031] The beneficial effects of the present invention are:
[0032] 1. The present invention provides a kind of hollow repair material in the field of building construction, the hollow repair material contains a variety of active ingredients, through the mutual coordination and compounding between components, especially the combination of silicate cement, sulphoaluminate cement, cellulose ether, tartaric acid and lithium carbonate, a synergistic effect is produced, which plays a role in improving bonding strength. After the inventor detects according to the detection method of JC / T2381-2016, the initial setting time of the hollow repair material is ≤30 minutes, the final setting time is ≤50 minutes, the compressive strength (6h) is ≥15MPa, the compressive strength (24h) is ≥20MPa, and the tensile bond strength (untreated 1d) is ≥0.6MPa, which fully meets the standard requirements. The hollow repair material has the advantages of high bonding strength, strong fluidity, rapid solidification, waterproof, anti-cracking, etc., which can not only effectively shorten the construction period, but also effectively reduce costs and reduce renovation costs.
[0033] 2. The present invention provides a method for preparing a hollowing repair material. The preparation method is simple and can be prepared and used on site, which can effectively shorten the construction period and reduce costs.
[0034] 3. The present invention also provides a hollow repair method, which uses the hollow repair material for repair, and has the effects of simple and fast construction and good pasting quality. DETAILED DESCRIPTION
[0035] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0036] Example 1
[0037] A hollow repair material in the field of building construction, the hollow repair material consisting of powder and emulsion;
[0038] The powder is composed of the following components in percentage by weight: 30% of general silicate cement, 60% of rapid hardening sulphoaluminate cement, 9.72% of quartz powder, 0.02% of cellulose ether, 0.1% of tartaric acid, 0.05% of polycarboxylic acid water reducer, 0.1% of polyether defoamer and 0.01% of lithium carbonate.
[0039] The emulsion is an acrylic emulsion with a concentration of 30 wt%.
[0040] The weight ratio of the powder to the emulsion is 1:0.38.
[0041] The preparation method of the hollow drum repair material comprises the following steps:
[0042] S1. According to the ratio of the hollow drum repair material, weigh each component for later use;
[0043] S2. Add the emulsion into the container, then add the powder, stir at a speed of 145 r / min for 3 minutes, and stir evenly to obtain the hollow repair material.
[0044] The hollow repair material in this embodiment was tested according to the testing method of JC / T2381-2016, and the results are shown in the following table:
[0045] Table 1: Test results of Example 1
[0046]
[0047]
[0048] Example 2
[0049] A hollow repair material in the field of building construction, the hollow repair material consisting of powder and emulsion;
[0050] The powder is composed of the following components in percentage by weight: 10% of general silicate cement, 80% of rapid hardening sulphoaluminate cement, 9.58% of quartz powder, 0.1% of cellulose ether, 0.01% of tartaric acid, 0.2% of polycarboxylic acid water reducer, 0.01% of polyether defoamer and 0.1% of lithium carbonate.
[0051] The emulsion is an acrylic emulsion with a concentration of 10 wt%.
[0052] The weight ratio of the powder to the emulsion is 1:0.34.
[0053] The preparation method of the hollow drum repair material comprises the following steps:
[0054] S1. According to the ratio of the hollow drum repair material, weigh each component for later use;
[0055] S2. Add the emulsion into the container, then add the powder, stir at a speed of 135 r / min, stir for 2 minutes, and obtain the hollow repair material after stirring evenly.
[0056] The hollow repair material in this embodiment was tested according to the testing method of JC / T2381-2016, and the results are shown in the following table:
[0057] Table 2: Test results of Example 2
[0058] project Technical indicators Detection value Setting time: initial setting ≤30min 20 Setting time: Final setting ≤50min 44 Tensile bond strength untreated 1d (MPa) ≥0.6 0.96 6h compressive strength (MPa) ≥15 16.8 24h compressive strength (MPa) ≥20 27
[0059] Example 3
[0060] A hollow repair material in the field of building construction, the hollow repair material consisting of powder and emulsion;
[0061] The powder is composed of the following components in percentage by weight: 20% of general silicate cement, 70% of rapid hardening sulphoaluminate cement, 9.56% of quartz powder, 0.06% of cellulose ether, 0.06% of tartaric acid, 0.2% of polycarboxylic acid water reducer, 0.06% of polyether defoamer and 0.06% of lithium carbonate.
[0062] The emulsion is an acrylic emulsion with a concentration of 20 wt%.
[0063] The weight ratio of the powder to the emulsion is 1:0.36.
[0064] The preparation method of the hollow drum repair material comprises the following steps:
[0065] S1. According to the ratio of the hollow drum repair material, weigh each component for later use;
[0066] S2. Add the emulsion into the container, then add the powder, stir at a speed of 140 r / min for 3 minutes, and stir evenly to obtain the hollow repair material.
[0067] The hollow repair material in this embodiment was tested according to the testing method of JC / T2381-2016, and the results are shown in the following table:
[0068] Table 3: Test results of Example 3
[0069] project Technical indicators Detection value Setting time: initial setting ≤30min 24 Setting time: Final setting ≤50min 46 Tensile bond strength untreated 1d (MPa) ≥0.6 1.15 6h compressive strength (MPa) ≥15 16.2 24h compressive strength (MPa) ≥20 25.3
[0070] Example 4
[0071] A hollow repair material in the field of building construction, the hollow repair material consisting of powder and emulsion;
[0072] The powder is composed of the following components in percentage by weight: 19.65% of general silicate cement, 65% of rapid hardening sulphoaluminate cement, 15% of quartz powder, 0.08% of cellulose ether, 0.04% of tartaric acid, 0.12% of polycarboxylic acid water reducer, 0.08% of polyether defoamer and 0.03% of lithium carbonate.
[0073] The emulsion is an acrylic emulsion with a concentration of 30 wt%.
[0074] The weight ratio of the powder to the emulsion is 1:0.37.
[0075] The preparation method of the hollow drum repair material comprises the following steps:
[0076] S1. According to the ratio of the hollow drum repair material, weigh each component for later use;
[0077] S2. Add the emulsion into the container, then add the powder, stir at a speed of 145 r / min, stir for 2.5 minutes, and after stirring evenly, the hollow repair material can be obtained.
[0078] The hollow repair material in this embodiment was tested according to the testing method of JC / T2381-2016, and the results are shown in the following table:
[0079] Table 4: Test results of Example 4
[0080] project Technical indicators Detection value Setting time: initial setting ≤30min 27.8 Setting time: Final setting ≤50min 49 Tensile bond strength untreated 1d (MPa) ≥0.6 1.32 6h compressive strength (MPa) ≥15 15.5 24h compressive strength (MPa) ≥20 23.7
[0081] Example 5
[0082] A hollow repair material in the field of building construction, the hollow repair material consisting of powder and emulsion;
[0083] The powder is composed of the following components in percentage by weight: 19.6% of general silicate cement, 75% of rapid hardening sulphoaluminate cement, 5% of quartz powder, 0.04% of cellulose ether, 0.08% of tartaric acid, 0.16% of polycarboxylic acid water reducer, 0.04% of polyether defoamer and 0.08% of lithium carbonate.
[0084] The emulsion is an acrylic emulsion with a concentration of 20 wt%.
[0085] The weight ratio of the powder to the emulsion is 1:0.37.
[0086] The preparation method of the hollow drum repair material comprises the following steps:
[0087] S1. According to the ratio of the hollow drum repair material, weigh each component for later use;
[0088] S2. Add the emulsion into the container, then add the powder, stir at a speed of 135 r / min for 3 minutes, and stir evenly to obtain the hollow repair material.
[0089] The hollow repair material in this embodiment was tested according to the testing method of JC / T2381-2016, and the results are shown in the following table:
[0090] Table 5: Test results of Example 5
[0091] project Technical indicators Detection value Setting time: initial setting ≤30min 24.4 Setting time: Final setting ≤50min 47 Tensile bond strength untreated 1d (MPa) ≥0.6 1.14 6h compressive strength (MPa) ≥15 16.3 24h compressive strength (MPa) ≥20 24.7
[0092] Comparative Example
[0093] In order to verify the performance of the hollow repair material of the present invention, the hollow repair material in Example 3 and the commercially available conventional hollow repair material (main components and contents of which are 60% general silicate cement, 20% rapid hardening sulphoaluminate cement, and 30% quartz powder) were tested according to the testing method of JC / T2381-2016. The test results are as follows:
[0094] Table 6: Comparative test results
[0095]
[0096] It can be seen from the above table that the hollow repair material of the present application has better construction performance than commercially available products, and has the advantages of higher bonding strength and compressive strength.
[0097] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A hollow repair material in the field of building construction, characterized in that: The hollow repair material is composed of powder and emulsion, and the weight ratio of the powder to the emulsion is 1:0.34-0.38; The powder is composed of the following components in weight percentage: 10-30% of silicate cement, 60-80% of sulphoaluminate cement, 5-15% of quartz powder, 0.02-0.1% of cellulose ether, 0.01-0.1% of tartaric acid, 0.05-0.2% of water reducing agent, 0.01-0.1% of defoaming agent and 0.01-0.1% of lithium carbonate.
2. The hollow drum repair material according to claim 1, characterized in that: The silicate cement is general silicate cement, and the sulphoaluminate cement is fast-hardening sulphoaluminate cement.
3. The hollow drum repair material according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent.
4. The hollow drum repair material according to claim 1, characterized in that: The defoamer is a polyether defoamer.
5. The hollow drum repairing material according to claim 1, characterized in that: The emulsion is an acrylic emulsion with a concentration of 10-30 wt%.
6. A method for preparing a hollow drum repair material, characterized in that: The following steps are involved: S1. According to the proportion of the hollow drum repair material according to any one of claims 1 to 5, weigh each component for later use; S2. Add the emulsion into a container, then add the powder, and stir evenly to obtain the hollow repair material.
7. The preparation method according to claim 6, characterized in that: In step S2, the stirring speed is 135-145 r / min, the stirring time is 2-3 minutes, and the mixture can be used for construction after being stirred evenly.
8. A hollow repair method in the field of building construction, characterized in that: Use the hollow repair material described in any one of claims 1 to 5 to repair hollows.
9. The hollow drum repairing method according to claim 8, characterized in that: The hollowing repair material is used to repair hollowing of ceramic tiles or hollowing of wall and floor mortar.