Method for preparing inner-cooling cutter by jointly adding LaB6 based on additive manufacturing
Through the combination of additive manufacturing technology and LaB6 powder, the manufacturing problems of complex internal cooling structures are solved, the mechanical properties of internal cooling tools are improved, and the forming and efficient cooling of complex internal cooling structures such as special-shaped cross-sections are achieved.
Patent Information
- Application Number
- CN202410996971.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The prior art is difficult to manufacture complex internal cooling tools with internal cooling structures, and cannot meet the needs of complex internal cooling structures such as special-shaped cross-sections.
Adopting additive manufacturing technology, combining high-speed steel powder and LaB6 powder, the molding of complex internal cooling structures is achieved through alternating additive manufacturing and sintering, and the rare earth elements and B elements in LaB6 powder are suppressed and the sintering temperature is reduced. , improve the relative density of internal cooling tools.
The manufacturing of complex internal cooling structures such as special-shaped cross-sections is realized, and the mechanical properties of internal cooling tools are improved, including high hardness and tensile strength, meeting the needs of complex internal cooling structures.
Smart Images

Figure CN118905225A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a method for preparing an internally cooled tool based on additive manufacturing and combined addition of LaB6. Background Art
[0002] The metal cutting process will generate a lot of cutting heat. Cutting tools with internal cooling structure (internal cooling tools for short) can take away a lot of cutting heat through coolant. Compared with external cooling, internal cooling tools can directly deliver coolant to the tool processing area, where heat is efficiently and quickly dissipated. This cooling method can break through the physical limits of traditional overflow coolant transmission and heat dissipation, which is conducive to extending tool life to a greater extent and improving surface processing quality.
[0003] However, the current technology for preparing internally cooled tools is limited by machining processes or mold injection processes, and can only produce simple internal cooling channels through extrusion molding or later drilling, which cannot meet the requirements of internally cooled tools for complex internal cooling structures such as special-shaped sections.
[0004] Based on this, there is an urgent need for a method of preparing internally cooled tools based on additive manufacturing and the combined addition of LaB6 to solve the above technical problems. Summary of the invention
[0005] The present invention provides a method for preparing an internally-cooled tool based on additive manufacturing and combined addition of LaB6, which can meet the requirements of the internally-cooled tool for complex internally-cooled structures such as special-shaped cross-sections.
[0006] The embodiment of the present invention provides a method for preparing an internally cooled tool based on additive manufacturing and adding LaB6, comprising:
[0007] Obtaining target metal powder and target adhesive; wherein the target metal powder includes high-speed steel powder and LaB6 powder;
[0008] Alternately performing additive manufacturing on the target metal powder and the target adhesive to obtain a calcined body;
[0009] The pre-burnt body is sintered to obtain an internally cooled tool.
[0010] It can be seen from the above scheme that the method for preparing an internally cooled tool based on additive manufacturing and adding LaB6 provided by the present invention alternately performs additive manufacturing on the target metal powder and the target adhesive, and can have a very high degree of freedom in molding based on the molding principle of layer-by-layer stacking of additive manufacturing, thereby being able to realize the integrated manufacturing of complex internally cooled structures such as special-shaped sections; further, the target metal powder includes LaB6 powder, so that the rare earth element La in the LaB6 powder can be used to inhibit the segregation of carbides in the high-speed steel powder, and the B element in the LaB6 powder can be used to produce a eutectic reaction with the high-speed steel powder to reduce the sintering temperature, thereby generating more liquid fluid to fill the pores between the high-speed steel powders, which can increase the relative density of the internally cooled tool, eliminate the pores, and ultimately improve the mechanical properties of the internally cooled tool. Therefore, the above technical scheme can meet the requirements of the internally cooled tool for complex internally cooled structures such as special-shaped sections. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0012] Figure 1 A schematic flow chart of a method for preparing an internally cooled tool by adding LaB6 based on additive manufacturing provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0013] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0014] See also Figure 1 The embodiment of the present invention provides a method for preparing an internally cooled tool based on additive manufacturing and adding LaB6, the method comprising:
[0015] Step S1, obtaining target metal powder and target adhesive; wherein the target metal powder includes high-speed steel powder and LaB6 powder;
[0016] Step S2, alternately performing additive manufacturing on the target metal powder and the target adhesive to obtain a calcined body;
[0017] Step S3, sintering the pre-burnt body to obtain an internally cooled tool.
[0018] In this embodiment, the target metal powder and the target adhesive are alternately additively manufactured, which can be based on the molding principle of additive manufacturing layer by layer stacking, with extremely high molding freedom, so that the integrated manufacturing of complex internal cooling structures such as special-shaped sections can be achieved; further, the target metal powder includes LaB6 powder, so that the rare earth element La in the LaB6 powder can be used to suppress the carbide segregation in the high-speed steel powder, and the B element in the LaB6 powder can be used to produce a eutectic reaction with the high-speed steel powder to reduce the sintering temperature, so that more liquid fluid can be generated to fill the pores between the high-speed steel powders, which can increase the relative density of the internal cooling tool, eliminate the pores, and ultimately improve the mechanical properties of the internal cooling tool. Therefore, the above technical solution can meet the requirements of the internal cooling tool for complex internal cooling structures such as special-shaped sections.
[0019] High-speed steel is an important high-end tool material with the characteristics of high hardness, high red hardness, high wear resistance, etc. It plays an important role in the field of tool manufacturing and metal processing, and is widely used in the manufacture of tools such as tools, drills, planers, milling cutters, etc. In metal cutting, high-speed steel tools can efficiently cut various metal materials, such as steel, aluminum alloy, stainless steel, etc., and provide high precision and high surface quality for workpiece processing. In the field of mold manufacturing, high-speed steel can be used to manufacture mold cores, mold cavities and other components, and bear high-strength and high-wear-resistant working environments. In mechanical processing, the high-speed cutting performance of high-speed steel tools can improve production efficiency, reduce processing costs, and meet the needs of industrial production for efficient processing.
[0020] In some embodiments, the high speed steel powder is M2 high speed steel powder.
[0021] M2 high-speed steel has excellent hardness, wear resistance and thermal stability. The composition design and reasonable element ratio are the basis of its excellent performance. Its main components include carbon, molybdenum, vanadium, chromium and other elements. Among them, C is the key element to improve the hardness and wear resistance of steel; the addition of Mo can improve the hardness and thermal stability; V can enhance the rigidity and wear resistance; Cr can improve the corrosion resistance. As an important alloying element in high-speed steel, W can significantly improve the hardness, thermal stability and wear resistance of high-speed steel. During the preparation process, M2 high-speed steel needs to undergo a strict heat treatment process, which includes heating, insulation and cooling steps to adjust the structure and performance of the material. Through appropriate heat treatment process, M2 high-speed steel can obtain ideal hardness, toughness and wear resistance, so as to meet the requirements of different working conditions. Because of its high carbon content and alloy composition (W, Mo, Cr, V, etc.), it is very easy to cause element segregation in the traditional preparation process, and it is easy to produce coarse primary carbides (such as M2C, M6C, etc.) and large-sized inclusions, which leads to premature failure of products such as cutting tools during use.
[0022] In order to solve this technical problem, it is possible to consider adding the rare earth element La to the high-speed steel powder. The rare earth element La can form a compound with a higher melting point in the steel, precipitate before the molten steel solidifies, and be distributed in the molten steel as fine particles, which can serve as a heterogeneous nucleation center to reduce the supercooling of the molten steel crystallization, thereby refining the solidification structure of the steel and reducing segregation. In addition, rare earths, as surface active elements, can reduce the surface tension of the molten steel, thereby reducing the work required to form a critical size of crystal nuclei and increasing the crystallization core. In addition, rare earths also play a role in purifying the steel body. After rare earths are added to the steel, they will first react with oxygen and sulfur in the molten steel to form rare earth oxides, oxysulfides, and sulfides to reduce their content, while inhibiting the segregation of these residual elements at the grain boundaries.
[0023] At the same time, considering the improvement of the mechanical properties of the internally cooled tool, its relative density can be increased, and the B element can distort the lattice and be activated when it produces a eutectic reaction with the sintered material. Therefore, the sintering temperature can be reduced, and the diffusion and sintering speed can be accelerated. If there is a suitable liquid fluid during sintering, it will often greatly promote the particle rearrangement and mass transfer process. Another mechanism of action of the B element is that it can produce liquid fluid at a lower temperature to promote sintering.
[0024] Therefore, after comprehensive consideration, LaB6 powder can be added to the high-speed steel powder to enhance the mechanical properties of the subsequent internally cooled tool.
[0025] In one embodiment of the present invention, the target metal powder includes two M2 high-speed steel powders of different particle sizes. This arrangement allows the powder with a smaller particle size to be filled into the gap between the powder with a larger particle size, and the powders with different particle sizes will produce different interfaces. Due to the interface effect, the subsequent sintering process will be accelerated, that is, it is beneficial to the subsequent sintering.
[0026] In one embodiment of the present invention, the parameters of the first particle size M2 high speed steel powder include: particle size range of 15 to 53 μm, D 50 The diameter of the alloy is 36.43 μm. The chemical composition is calculated by mass percentage: C content is 0.86%, Mn content is 0.35%, Cr content is 4.15%, Si content is 0.36%, V content is 4.10%, W content is 6.20%, Mo content is 5.00%, and the balance is Fe. The bulk density is 4.18 g / cm 3 , tap density is 4.8g / cm 3 ;
[0027] The parameters of the second particle size M2 high speed steel powder include: particle size range of 1 to 15 μm, D 50 The diameter of the alloy is 6.42 μm. The chemical composition is calculated by mass percentage, including C content of 0.87%, Mn content of 0.34%, Cr content of 4.23%, Si content of 0.45%, V content of 1.90%, W content of 6.21%, Mo content of 5.17%, and the balance of Fe. The bulk density is 4.12 g / cm 3 , tap density is 4.99g / cm 3 ;
[0028] The mass fraction of the M2 high speed steel powder with the first particle size is 63.17%, and the mass fraction of the M2 high speed steel powder with the second particle size is 36.83%.
[0029] In this embodiment, by limiting the specific parameters of two M2 high-speed steel powders with different particle sizes, the optimal mixing ratio (i.e., mass fraction) of the two can be calculated, so that the maximum relative theoretical packing density of the powder bed can be obtained, thereby maximizing the relative density of the internally cooled tool.
[0030] In one embodiment of the present invention, the mass fractions of two M2 high-speed steel powders with different particle sizes are obtained by dividing the D 50 The tap density is input into a preset mathematical calculation model to obtain the result. The mathematical calculation model is not limited here, and the mathematical calculation model is obtained by Python programming.
[0031] In some embodiments, the target metal powder is obtained by high-energy ball milling (the ball milling method is dry mixing, and the ball milling time is 48 hours) of M2 high-speed steel powder with a first particle size of 63.17% by mass and M2 high-speed steel powder with a second particle size of 36.83% by mass, and then drying and sieving.
[0032] In one embodiment of the present invention, the chemical composition of the target adhesive includes 17.54% by mass of 4-pentyn-2-ol, 1.13% by mass of isopropanol, 3.42% by mass of ethylene glycol, 76.79% by mass of ethylene glycol monobutyl ether, 1% by mass of pentaethylenehexamine, and 0.12% by mass of tris(2-aminoethyl)amine.
[0033] In this embodiment, the above chemical components do not contain harmful substances, and the target adhesive will not volatilize (therefore, it is necessary to remove the adhesive through subsequent drying), which will not cause harm to the environment and human body; and the target adhesive has good bonding properties and can firmly bond two M2 high-speed steel powders of different particle sizes together.
[0034] In one embodiment of the present invention, the parameters of additive manufacturing include: the thickness of each layer of target metal powder is 80 μm, the D 50 The diameter is 24.81 μm and the tap density is 5.36 g / cm 3 , the saturation of the target adhesive is 10.95%.
[0035] It is understandable that some parameters of additive manufacturing are obtained by constructing a three-dimensional model of the workpiece to be processed using modeling software and slicing the three-dimensional model of the workpiece to be processed in computer slicing software, while other parameters are set manually.
[0036] In one embodiment of the present invention, after obtaining the calcined body and before sintering the calcined body, the method further comprises:
[0037] The pre-burned body is heated and cured and dried to remove the glue in sequence; wherein the heating temperature is 200°C, the heating time is 4 to 5 hours, the drying temperature is 600°C, and the drying time is 1 to 2 hours.
[0038] In this embodiment, the pre-burned body is heated and cured so that the pre-burned body has a certain strength and a solid shape; and the target adhesive is removed by drying the pre-burned body after heating and curing to ensure the mechanical properties of the internally cooled tool obtained later.
[0039] In one embodiment of the present invention, after sintering the pre-burnt body, the method further comprises:
[0040] The sintered finished product is cleaned and polished in sequence; wherein, the cleaning time is 0.5 to 1 hour, and the cleaning medium is anhydrous ethanol.
[0041] In some embodiments, cleaning may be ultrasonic cleaning; polishing may be grinding the sintered finished product on #240, #400, #600, #800, #1000, #1200, #1500, #2000, and 3000 sandpaper in sequence, and then polishing it with a diamond polishing agent, so as to obtain an internally cooled tool with good mechanical properties.
[0042] Furthermore, when sintering the pre-burned body, an optimized sintering process may be considered, which can increase the relative density of the internally cooled tool, eliminate pores, and ultimately improve the mechanical properties of the internally cooled tool.
[0043] In one embodiment of the present invention, the optimized sintering process is: sintering at a first preset temperature range for a first preset time in an inert gas atmosphere, increasing the sintering temperature to a second preset temperature range within a second preset time, and continuing to sinter for a third preset time in a vacuum atmosphere.
[0044] In some embodiments, the inert gas may be argon, helium and nitrogen, preferably argon, because nitrogen may form nitrides on the metal surface during sintering, thereby affecting the mechanical properties of the internally cooled tool, while helium is relatively expensive.
[0045] In this embodiment, after the first sintering process is completed, the introduction of argon during the cooling process can effectively prevent the oxidation reaction between oxygen and metal powder, reduce the oxidation degree of the sintered part, maintain the stability of the material composition and performance, and improve the quality and surface finish of the sintered part. At the same time, since argon has good thermal conductivity, the introduction of argon can accelerate the cooling speed of the sintered part, shorten the sintering time, improve the sintering efficiency, and reduce the production cost. In addition, continuing sintering in a vacuum atmosphere can effectively increase the relative density of the internally cooled tool and eliminate porosity.
[0046] In one embodiment of the present invention, the first preset temperature range is 1200-1280°C, the second preset temperature range is 1300-1380°C, the first preset time is 50-45 minutes, the second preset time is 3-6 minutes, and the third preset time is 10-15 minutes.
[0047] In this embodiment, the sintered part is first sintered within the first preset temperature range to form a matrix. During the sintering process, the connection between the powders will be partially liquefied, that is, the atoms or molecules on the surface of the powder particles will diffuse (i.e., form a fluid), so that the contact area between the particles is expanded. When the atoms or molecules between the particles diffuse to a certain extent, they will form a strong bond between the particles, thereby achieving fixation between the particles. However, at this time, since there is less fluid generated by liquefaction during the sintering process, the bonding strength between the powder particles is poor, and the relative density of the pre-sintered body is low. Next, the sintering temperature is quickly increased to the second preset temperature range within a very short time (i.e., the second preset time), and maintained for a short time (i.e., the third preset time), and a large amount of fluid generated in the matrix is used to fill the pores between the particles, so that a sintered product with a higher relative density can be obtained, that is, the mechanical properties, tensile strength and hardness of the internally cooled tool are improved.
[0048] Experiments show that the internally cooled tool produced by the method provided in the embodiment of the present invention has a relative density of up to 99.95%, a hardness of 52-54 HRC at room temperature, a tensile strength of 800-1200 MPa, and good mechanical properties.
[0049] In summary, the method provided in the embodiment of the present invention improves the mechanical properties of the internally cooled tool in the following ways: 1) adding LaB6 powder to the high-speed steel powder; 2) the target metal powder includes two M2 high-speed steel powders with different particle sizes, and the optimal mixing ratio of the two is further determined; 3) the pre-sintered body is sintered using the optimized sintering process.
[0050] It should be noted that, in the present invention, relational terms such as first and second are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0051] Finally, it should be noted that the above is only a preferred embodiment of the present invention, which is only used to illustrate the technical solution of the present invention, and is not used to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A method for preparing an internally cooled tool based on additive manufacturing and combined addition of LaB6, characterized in that: include: Obtaining target metal powder and target adhesive; wherein the target metal powder includes high-speed steel powder and LaB6 powder; Alternately performing additive manufacturing on the target metal powder and the target adhesive to obtain a calcined body; The pre-burnt body is sintered to obtain an internally cooled tool.
2. The method according to claim 1, characterized in that: The target metal powder includes two types of M2 high speed steel powders with different particle sizes.
3. The method according to claim 2, characterized in that The parameters of the first particle size M2 high speed steel powder include: particle size range of 15 to 53 μm, D 50 The diameter of the alloy is 36.43 μm. The chemical composition is calculated by mass percentage: C content is 0.86%, Mn content is 0.35%, Cr content is 4.15%, Si content is 0.36%, V content is 4.10%, W content is 6.20%, Mo content is 5.00%, and the balance is Fe. The bulk density is 4.18 g / cm 3 , tap density is 4.8g / cm 3 ; The parameters of the second particle size M2 high speed steel powder include: particle size range of 1 to 15 μm, D 50 The diameter of the alloy is 6.42 μm. The chemical composition is calculated by mass percentage, including C content of 0.87%, Mn content of 0.34%, Cr content of 4.23%, Si content of 0.45%, V content of 1.90%, W content of 6.21%, Mo content of 5.17%, and the balance of Fe. The bulk density is 4.12 g / cm 3 , tap density is 4.99g / cm 3 ; The mass fraction of the M2 high speed steel powder with the first particle size is 63.17%, and the mass fraction of the M2 high speed steel powder with the second particle size is 36.83%.
4. The method according to claim 3, characterized in that The mass fractions of two M2 high-speed steel powders with different particle sizes were calculated by dividing their D 50 The tap density is input into the preset mathematical calculation model.
5. The method according to claim 3, characterized in that: The particle size of the LaB6 powder is 300 to 500 nm.
6. The method according to claim 3, characterized in that The mass ratio of the LaB6 powder to the high-speed steel powder is (0.1-0.5):
100.
7. The method according to claim 2, characterized in that The chemical composition of the target adhesive includes 17.54% by mass of 4-pentyn-2-ol, 1.13% by mass of isopropanol, 3.42% by mass of ethylene glycol, 76.79% by mass of ethylene glycol monobutyl ether, 1% by mass of pentaethylenehexamine and 0.12% by mass of tris(2-aminoethyl)amine.
8. The method according to claim 2, characterized in that: The parameters of the additive manufacturing include: the thickness of each layer of the target metal powder is 80 μm, the D 50 The diameter is 24.81 μm and the tap density is 5.36 g / cm 3 , the saturation of the target adhesive is 10.95%.
9. The method according to claim 2, characterized in that: After obtaining the calcined body and before sintering the calcined body, the method further comprises: The pre-calcined body is heated and cured and dried to remove the glue in sequence; wherein the heating temperature is 200° C., the heating time is 4 to 5 hours, the drying temperature is 600° C., and the drying time is 1 to 2 hours.
10. The method according to claim 2, characterized in that After sintering the pre-calcined body, the method further comprises: The sintered finished product is cleaned and polished in sequence; wherein, the cleaning time is 0.5 to 1 hour, and the cleaning medium is anhydrous ethanol.
Citation Information
Patent Citations
Three-dimensional printer and printing method thereof
CN105921751A
Magnesium alloy 3D additive manufacturing high-viscosity full-liquid-phase sintering method
CN112974836A
Binder jet sintering additives and methods of use thereof
WO2019221999A1
KR20230121370A