Ceramic / metal interface bonding method based on binder spray molding
Through adhesive spray forming technology and intermediate layer coating, combined with casting technology, the problem of poor interface wetting of ceramic/metal bonding technology on complex shape parts is solved, and the integrated molding of ceramic/metal parts is realized, which improves resistance Wear corrosion resistance and service life.
Patent Information
- Application Number
- CN202410899201.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The existing ceramic/metal bonding technology is complex in technology and high in cost, making it difficult to meet the coating preparation of complex-shaped parts, especially in the inner cavity and runner area of complex structures, resulting in poor interface wetting and difficulty in achieving good bonding.
The ceramic shell is quickly prepared by adhesive spray molding technology, and the wettability of ceramics and metals is improved through intermediate layer coating. Combined with casting technology, the integrated molding of ceramics/metal parts is achieved. The specific steps include designing a castable hollow ceramic shell, using adhesive jet molding technology to manufacture the ceramic shell, performing curing, vacuum impregnation, drying and degreasing sintering, and then depositing a metal intermediate layer on the inner surface of the ceramic shell, and finally through casting. Fill in liquid metal and solidify with temperature control.
The castings that combine ceramic/metal interface improve the wear and corrosion resistance of the parts, enhance the service performance and life. They are suitable for complex components, with simple process and strong operability, and are suitable for various complex inner cavity and runner shapes. parts.
Smart Images

Figure CN118905241A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of casting, and more specifically, relates to a ceramic / metal interface bonding method based on binder injection molding. Background Art
[0002] With the improvement of science and technology, the working environment of industrial equipment has become more complex and diversified. Metal parts are widely used in various industrial equipment and structures. With the improvement of use requirements and the expansion of working environment, the performance of a single metal is usually unable to meet the needs of extreme and harsh working conditions. In view of the wear and corrosion resistance requirements of mechanical parts, the use of ceramic / metal materials is a feasible solution. The composite of metal and ceramic can effectively retain the toughness of metal materials and the wear and corrosion resistance of ceramic materials, and is an ideal material for mechanical parts.
[0003] Patent document CN114988918A discloses a method for surface metallization of alumina ceramics, in which metal powder, additives and organic carriers are mixed to form a metallization slurry, which is then printed onto an alumina ceramic substrate using a screen, followed by drying, gas-protected degreasing and sintering to obtain surface metallized alumina ceramics. The preparation process is complex and can only achieve ceramic / metal bonding of simple structures (this is because for complex structures, there are often areas that cannot be covered by screen printing, limiting the application).
[0004] Patent document CN102978616A discloses a centrifugal self-propagating method for preparing an aluminum oxide coating on the surface of a steel plate, using a flame powder spray gun to spray nickel-coated aluminum powder on the outer side of the roughened steel plate, and then the aluminum oxide coating is applied to the surface of the steel plate through a thermal reaction using a centrifugal turntable and aluminothermic flux provided by the device. It can only achieve ceramic / metal bonding of simple plate structures, which has great limitations (this is because for complex structures, there are often areas that cannot be sprayed by the spray gun, which limits the application).
[0005] There are great differences between metals and ceramics in terms of physical, chemical and mechanical properties, and the wettability of the interface is poor. Although the above method can achieve the combination of metal and ceramic, the process is complicated and the cost is high, and it is difficult to meet the coating preparation requirements of the inner cavity and flow channel of complex parts. Therefore, in order to achieve a good combination of ceramic / metal interfaces under complex shapes, it is necessary to explore a ceramic / metal parts preparation method with high production efficiency and simple preparation process. Summary of the invention
[0006] In view of the above defects or improvement needs of the prior art, the purpose of the present invention is to provide a ceramic / metal interface bonding method based on binder injection molding. Through the binder injection molding technology, a ceramic shell can be quickly and directly prepared, and then the wettability of ceramic and metal is improved by intermediate layer coating. Combined with casting technology, the integrated molding of ceramic / metal parts is realized. The obtained castings with ceramic / metal interface bonding have improved the wear and corrosion resistance of the metal compared to pure metal castings, which will greatly improve the performance and service life of the parts. It is also a major technological breakthrough in the manufacturing of mechanical parts.
[0007] To achieve the above object, according to the present invention, a ceramic / metal interface bonding method based on binder injection molding is provided, characterized in that it comprises the following steps:
[0008] S1 is based on 3D printing and designs a castable hollow ceramic shell according to the structure of the target casting;
[0009] S2 uses binder injection molding technology to 3D print the hollow ceramic shell to obtain a blank, and then successively undergoes curing, vacuum infiltration, drying and degreasing sintering to obtain a ceramic shell; wherein the degreasing sintering is used to remove the binder by sintering;
[0010] S3 deposits an intermediate layer containing a metal material on the inner surface of the ceramic shell by vacuum dipping or chemical plating;
[0011] S4 uses a casting method to fill the iron-based metal liquid into the interior of a ceramic shell with an intermediate layer deposited thereon. After temperature-controlled solidification and heat preservation treatment, a casting with a ceramic / metal interface bond can be obtained after cooling.
[0012] As a further preferred embodiment of the present invention, step S2 specifically comprises pre-mixing the ceramic powder to be printed with the sintering aid MnO2, and then 3D printing the obtained mixture using a binder injection molding technology to obtain a preform; wherein the mass proportion of the sintering aid MnO2 in the mixture is 6% to 10%, and the particle sizes of the sintering aid and the ceramic powder are both between 500 and 2000 meshes; preferably, the ceramic powder is alumina ceramic powder;
[0013] In step S2, the curing temperature used for curing is 160-220°C and the curing time is 2-3h;
[0014] The vacuum impregnation liquid used is TiO2 sol, with a solid content of 20-30wt%, an impregnation time of 90-120s, and an impregnation vacuum of 20-30KPa;
[0015] The process parameters of the debinding sintering are: heating from room temperature to 640-660°C at a heating rate of 2-4°C / min, and keeping warm for 60-90 minutes; then heating to 950-1050°C at a heating rate of 2-4°C / min; then heating to 1400-1450°C at a heating rate of 1-2°C / min, and keeping warm for 2-4 hours; finally cooling to room temperature with the furnace.
[0016] As a further preferred embodiment of the present invention, step S3 specifically uses a vacuum dip coating method, wherein the coating is a mixture of aggregate and a coating binder; wherein the coating binder is a silica sol with a solid content of 20 to 40 wt%; the aggregate is a metal element powder with a particle size of 1000 to 1200 meshes, and the melting point of the metal element is 1400 to 1800°C; the mass percentage of the aggregate in the coating is 40 to 60%; preferably, the metal element powder is nickel powder, chromium powder or titanium powder;
[0017] Step S3 specifically includes the following sub-steps:
[0018] S3.1 Stir the coating with a high-speed mixer at a speed of 1500-2000 r / min for 10-15 min, and then perform vacuum dipping; the vacuum degree of vacuum dipping is 20-40 KPa, and the dipping time is 20-40 s;
[0019] S3.2 Place the vacuum-coated ceramic shell in a vacuum environment with a vacuum degree of 20 to 40 KPa for 1 to 2 hours to completely precipitate the bubbles in the coating;
[0020] S3.3 drying the ceramic shell obtained in step S3.2 at a temperature of 40 to 60° C. for 18 to 24 hours;
[0021] S3.4 sintering the ceramic shell obtained in step S3.3 to sinter the coating; the process parameters of the sintering treatment are: heating from room temperature to 1200-1300°C at a heating rate of 2-4°C / min, keeping warm for 30-60 minutes, and finally cooling to room temperature with the furnace.
[0022] As a further preferred embodiment of the present invention, step S3 is specifically performed by chemical nickel plating, and the corresponding intermediate layer obtained is a metal nickel layer;
[0023] Step S3 specifically includes the following sub-steps:
[0024] S3-1 Use anhydrous ethanol as a cleaning agent to ultrasonically clean the ceramic shell for 15 to 30 minutes, and then change to deionized water as a cleaning agent to ultrasonically clean the ceramic shell for 5 to 20 minutes to ensure that all stains that have penetrated into the ceramic pores are removed;
[0025] S3-2: placing the ceramic shell treated in step S3-1 into a NaOH solution with a concentration of 500 to 800 g / L, roughening it at 40 to 60° C. for 30 to 60 min, and then ultrasonically cleaning it multiple times using deionized water as a detergent, each ultrasonic cleaning time being 20 to 40 min, and measuring the pH value of the solution after each cleaning until the pH drops to 7.4 to 7.6, ensuring that the roughening solution on the surface and in the ceramic pores is completely removed;
[0026] S3-3: Soak the ceramic shell treated in step S3-2 in a sensitizing solution for 10 to 25 minutes for sensitization treatment, and then rinse the ceramic shell under running deionized water for 20 to 30 seconds after sensitization;
[0027] S3-4: Soak the ceramic shell treated in step S3-3 in an activation solution for 15 to 25 minutes for activation treatment, and then rinse the ceramic shell under flowing deionized water for 20 to 30 seconds after activation; then, place the obtained ceramic shell in a NaH2PO2 solution with a concentration of 18 to 30 g / L and reduce it for 3 to 8 minutes;
[0028] S3-5 placing the ceramic shell treated in step S3-4 in a plating solution and performing chemical plating at a temperature of 60 to 80° C.; during the chemical plating process, stirring the plating solution at a uniform speed, and the plating time is 20 to 40 minutes;
[0029] After S3-6 nickel plating is completed, take out the ceramic shell, clean it, and keep it at 180-250℃ for 40-60min, and then cool it down with the furnace.
[0030] As a further preferred embodiment of the present invention, in step S4, the iron-based molten metal is 65Mn spring steel molten metal;
[0031] The casting is specifically gravity casting, and the pouring temperature used is 1600-1700° C.; or, the casting is specifically vacuum suction casting, and the pouring temperature used is 1550-1650° C., and the negative pressure used is -0.05--0.1 MPa.
[0032] As a further preferred embodiment of the present invention, in step S4, the ceramic shell is preheated at above 1200° C. for 30 to 60 minutes before being cast;
[0033] The temperature-controlled solidification and heat preservation treatment is specifically to cool the workpiece at a preset rate after pouring is completed, and in the range of 1600-1200°C, keep the temperature for 1-2 hours after each 100°C-200°C reduction until the temperature drops to 700-800°C, and finally cool to room temperature with the furnace; the preset rate is specifically 1-2°C / min.
[0034] Through the above technical scheme conceived by the present invention, compared with the prior art, the present invention uses the binder injection molding technology to quickly and directly prepare the ceramic shell, and then improves the wettability of ceramic and metal by intermediate layer coating, and combines the casting technology to achieve the integrated molding of ceramic / metal parts. The casting with ceramic / metal interface bonding obtained by the present invention has good interface bonding.
[0035] The method of the present invention is applicable to complex components, as long as a castable hollow ceramic shell can be formed, and it is applicable to various complex parts with complex inner cavities and flow channel shapes. In addition, the present invention realizes 3D printing through binder injection molding technology. On the one hand, the molding structure obtained by binder injection molding does not require support, and the shape of the printed shell material is more free, which is suitable for complex structures; on the other hand, the higher open porosity of the ceramic prepared by binder injection molding also facilitates the infiltration of metal into the ceramic shell. Different from the casting method of ceramic / metal integrated parts based on layered extrusion molding reported by the research group of the inventor of the present invention (see Chinese patent ZL 201910691963.3 for details), the binder injection molding technology used in the method of the present invention has greater technical flexibility in molding ceramic shells, and can design ceramic shells more freely without support, and can prepare large-size parts. In addition, the intermediate layer preparation methods such as dip coating and chemical plating used in the present invention are more suitable for complex ceramic internal cavities and have greater technical application potential.
[0036] Specifically, the present invention can achieve the following beneficial effects:
[0037] (1) The method of the present invention breaks through the design limit of existing ceramic / metal parts through the binder injection molding technology, can form any complex ceramic shell and combine the intermediate layer preparation with the metal liquid pouring to realize the integrated molding of ceramic / metal parts, and has a simple process and strong operability.
[0038] (2) The method of the present invention is based on vacuum dipping coating or chemical plating to prepare an intermediate transition layer (i.e., intermediate layer) on the surface of ceramics (e.g., alumina ceramics). The transition layer can be coated on the surface of a complex inner cavity flow channel. The coating is uniform and well bonded. The powder selected for the coating can preferably be nickel powder, chromium powder, titanium powder, or other metals with a melting point of 1400 to 1800°C. The method has universal applicability and can meet the needs of preparing metal, ceramic, and other coatings on ceramic surfaces.
[0039] (3) The method of the present invention is applicable to various casting methods such as gravity casting and vacuum casting, and can be flexibly selected according to actual needs. For example, low-pressure casting methods such as vacuum casting are particularly suitable for thin-walled ceramic / metal parts with a wall thickness not exceeding 1 mm, and gravity casting is suitable for ordinary ceramic / metal castings that have no requirements on wall thickness. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The flowchart of the method for combining iron-based metal and alumina ceramic based on binder injection molding technology in an embodiment of the present invention.
[0041] Figure 2 This is a cross-sectional view of a sample with a metal transition layer coated on the surface of an alumina ceramic according to Example 1. In this example, reference numeral 1 corresponds to the alumina substrate region, and reference numeral 2 corresponds to the metal transition layer (i.e., the intermediate layer containing a metal material).
[0042] Figure 3 is the contact angle between alumina ceramic and iron-based metal liquid before and after adding transition layer Cr. Figure 3 (a) is a comparison of the contact angles between alumina ceramics and iron-based metal liquid before and after adding a transition layer of Cr, obtained by using the sessile drop method (wherein the legend "Cr coating" corresponds to alumina ceramics with a transition layer of Cr, and the legend "alumina ceramics" corresponds to alumina ceramics without a transition layer); Figure 3 (b) is an optical photograph of the initial state of alumina ceramics and iron-based metal liquid when there is no transition layer; Figure 3 (b1) is an optical photograph of the steady state of alumina ceramics and iron-based metal liquid without a transition layer; Figure 3 (c) is an optical photograph of the initial state of alumina ceramics and iron-based molten metal when the transition layer Cr is added; Figure 3 (c1) is an optical photograph of the steady state of alumina ceramics and iron-based molten metal when the transition layer Cr is added.
[0043] Figure 4 This is a diagram of the interface structure of the alumina ceramic without a transition layer involved in Comparative Example 1 after pouring with the iron-based metal liquid.
[0044] Figure 5 The interface structure and element distribution of the alumina ceramic with a Cr transition layer added in Example 1 after casting with the iron-based metal liquid. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0046] In general, the ceramic / metal interface bonding method based on binder injection molding in the present invention includes the following steps: (1) designing a castable hollow complex ceramic shell according to requirements; (2) mixing ceramic powder and sintering aids and sieving and drying; (3) preparing a hollow ceramic shell blank by binder injection molding technology, and performing solidification, vacuum infiltration, drying and degreasing sintering; (4) preparing an intermediate transition layer, coating the obtained ceramic shell with the intermediate transition layer, drying and sintering; (5) using a casting process (such as gravity casting, vacuum suction casting, etc.) to fill the iron-based metal liquid into the interior of the ceramic shell plated with the transition layer, and perform temperature-controlled solidification and heat preservation treatment, and finally achieve good interface bonding.
[0047] The following are specific embodiments:
[0048] Example 1
[0049] This embodiment provides a method for bonding iron-based metal and alumina ceramic based on binder injection molding technology, which specifically includes the following steps:
[0050] The first step is to manufacture the hollow ceramic shell by using a binder injection molding technology. Specifically, the preparation of the ceramic shell includes the following steps:
[0051] (1) Add 6 wt% of 500 mesh MnO2 sintering aid to 500 mesh alumina ceramic powder and mix for 4 h using an automatic powder mixer;
[0052] (2) The ceramic shell is integrally formed by using a binder injection molding technology, and the blank is cured at 160°C for 2 hours. The binder used in the binder injection molding technology is a phenolic resin binder, and the detailed parameter conditions used in the injection molding are: the layer height is 0.15 mm, and the binder saturation is 100%.
[0053] (3) vacuum impregnating the solidified green body with a TiO2 sol having a solid content of 20% for 90 seconds at a vacuum degree of 20 KPa, thereby strengthening the green body;
[0054] (4) drying the impregnated ceramic shell at 60° C. for 24 h until it is completely dehydrated;
[0055] (5) Degreasing and sintering the infiltrated and dried ceramic shell, the sintering parameters are set as follows: heating from room temperature to 640°C at a heating rate of 2°C / min, keeping the temperature for 60 min, then heating to 950°C at a heating rate of 2°C / min, reducing the heating rate to 1°C / min to 1400°C, keeping the temperature for 2 h, and finally cooling to room temperature with the furnace;
[0056] The second step is to prepare the middle layer by vacuum dipping coating. The binder of the coating is silica sol with a solid content of 20%. The aggregate is chromium powder with a particle size of 1000 mesh and the aggregate accounts for 40wt%. The preparation process includes the following sub-steps:
[0057] (1) The coating was stirred at a speed of 1500 r / min for 10 min using a high-speed stirrer and then dip-coated. The dipping vacuum was 20 KPa and the dipping time was 20 s.
[0058] (2) After dip coating, the ceramic shell is placed in a vacuum reactor at a vacuum degree of 20 KPa for 1 hour to ensure that the bubbles in the coating are completely precipitated;
[0059] (3) Drying the ceramic shell in a drying oven at 40° C. for 18 h;
[0060] (4) The process parameters for sintering the coating after drying are: heating from room temperature to 1200°C at a heating rate of 3°C / min, keeping the temperature for 30 min, and finally cooling to room temperature in the furnace. The resulting coating thickness is 200 μm.
[0061] In the third step, the sintered coated ceramic shell is buried in silica sand, with gates and risers reserved. It is preheated to 1200°C and kept warm for 30 minutes. The pouring temperature is 1600°C. After pouring, the product is kept warm at 1500°C, 1400°C, 1300°C and 1200°C for 1 hour respectively, with a cooling rate of 1°C / min in the middle. It is then cooled to 700°C at a rate of 1°C / min, and finally cooled to room temperature with the furnace.
[0062] The fourth step is to take out the casting after it cools down and cut off the pouring system part to obtain the alumina / iron composite casting.
[0063] The sample obtained in the second step of Example 1 was characterized by SEM. Figure 2 As shown, it is not difficult to see that after sintering, the Cr coating is well bonded to the alumina ceramic substrate without obvious cracks, and the coating is dense and uniform, indicating that the dip coating and sintering effect is good.
[0064] In addition, the sample obtained in the fourth step of Example 1 was characterized by SEM. Figure 5 As shown, it is not difficult to see that after adding the Cr intermediate layer and then gravity casting, the ceramic / metal sample has no obvious cracks at the bonding interface and is tightly bonded. In addition, an obvious Cr intermediate layer can be observed under surface scanning analysis, which proves the significant effect of the intermediate layer on the ceramic / metal interface bonding.
[0065] Comparative Example 1
[0066] This comparative example 1 does not contain the preparation of the intermediate layer, and specifically includes the following steps:
[0067] The first step is to manufacture the hollow ceramic shell by using a binder injection molding technology. Specifically, the preparation of the ceramic shell includes the following steps:
[0068] (1) Add 6 wt% of 500 mesh MnO2 sintering aid to 500 mesh alumina ceramic powder and mix for 4 h using an automatic powder mixer;
[0069] (2) The ceramic shell is integrally formed by using a binder injection molding technology, and the blank is cured at 160°C for 2 hours. The binder used in the binder injection molding technology is a phenolic resin binder, and the detailed parameter conditions used in the injection molding are: the layer height is 0.15 mm, and the binder saturation is 100%.
[0070] (3) vacuum impregnating the solidified green body with a TiO2 sol having a solid content of 20% for 90 seconds at a vacuum degree of 20 KPa, thereby strengthening the green body;
[0071] (4) drying the impregnated ceramic shell at 60° C. for 24 h until it is completely dehydrated;
[0072] (5) Degreasing and sintering the infiltrated and dried ceramic shell, the sintering parameters are set as follows: heating from room temperature to 640°C at a heating rate of 2°C / min, keeping the temperature for 60 min, then heating to 950°C at a heating rate of 2°C / min, reducing the heating rate to 1°C / min to 1400°C, keeping the temperature for 2 h, and finally cooling to room temperature with the furnace;
[0073] Step 2: bury the sintered ceramic shell in silica sand, reserve the pouring gate and riser, preheat to 1200℃, keep warm for 30 minutes, pouring temperature is 1600℃, keep the product at 1500℃, 1400℃, 1300℃ and 1200℃ for 1h after pouring, the cooling rate in the middle is 1℃ / min, then cool to 700℃ at a rate of 1℃ / min, and finally cool to room temperature with the furnace.
[0074] The third step is to take out the casting after it cools down and cut off the pouring system part to obtain the alumina / iron composite casting.
[0075] The sample obtained in the third step of Comparative Example 1 was characterized by SEM. Figure 4 As shown, it is not difficult to see that there are obvious cracks at the ceramic / metal gravity casting interface without an intermediate layer, and the interface front is severely oxidized, which has no application value.
[0076] The sample obtained in the first step of Comparative Example 1 and the sample obtained in the second step of Example 1 were tested for surface contact angle with the iron-based molten metal. The results are as follows: Figure 3As shown, it is not difficult to see that the contact angle of the sample with the added Cr intermediate layer with the iron-based metal liquid is reduced from 98.9° to 78.4° compared with the sample without the intermediate layer, that is, the interface changes from non-wetting (contact angle > 90°) to wetting (contact angle < 90°), which also proves the important role of the intermediate layer in the ceramic / metal interface bonding.
[0077] Example 2
[0078] This embodiment provides a method for bonding iron-based metal and alumina ceramic based on binder injection molding technology, which specifically includes the following steps:
[0079] The first step is to manufacture the hollow ceramic shell by using a binder injection molding technology. Specifically, the preparation of the ceramic shell includes the following steps:
[0080] (1) Add 8 wt% of 1250 mesh MnO2 sintering aid to 1250 mesh alumina ceramic powder and mix for 4 hours using an automatic powder mixer;
[0081] (2) The ceramic shell is integrally formed by using a binder injection molding technology, and the blank is cured at 190°C for 2.5 hours. The binder used in the binder injection molding technology is a phenolic resin binder, and the detailed parameter conditions used in the injection molding are: the layer height is 0.1 mm, and the binder saturation is 120%.
[0082] (3) vacuum impregnating the solidified preform with a TiO2 sol having a solid content of 25% for 105 seconds at a vacuum degree of 25 KPa;
[0083] (4) drying the impregnated ceramic shell at 60° C. for 24 h until it is completely dehydrated;
[0084] (5) Degreasing and sintering the infiltrated and dried ceramic shell, the sintering parameters are set as follows: heating from room temperature to 650°C at a heating rate of 3°C / min, keeping the temperature for 75 min, then heating to 1000°C at a heating rate of 3°C / min, reducing the heating rate to 1.5°C / min to 1425°C, keeping the temperature for 3 h, and finally cooling to room temperature in the furnace;
[0085] The second step is to prepare the middle layer by vacuum dipping coating. The binder of the coating is silica sol with a solid content of 30%. The aggregate is titanium powder with a particle size of 1200 mesh and the aggregate accounts for 60wt%. The preparation process includes the following sub-steps:
[0086] (1) The coating was stirred at a speed of 2000 r / min for 15 min using a high-speed stirrer and then dip-coated. The dipping vacuum was 40 KPa and the dipping time was 40 s.
[0087] (2) After dip coating, the ceramic shell is placed in a vacuum reactor at a vacuum degree of 40 KPa for 2 h to ensure that the bubbles in the coating are completely precipitated;
[0088] (3) Drying the ceramic shell in a drying oven at 60° C. for 24 h;
[0089] (4) The process parameters for sintering the coating after drying are: heating from room temperature to 1300°C at a heating rate of 3°C / min, keeping the temperature for 60 min, and finally cooling to room temperature in the furnace. The resulting coating thickness is 250 μm.
[0090] The third step is to place the sintered coated ceramic shell in a vacuum chamber, preheat to 1200°C, keep warm for 45 minutes, use a negative pressure of -0.05MPa for vacuum casting, vacuum cast 65Mn spring steel liquid, and pour at 1550°C. After pouring, keep the parts at 1400°C and 1200°C for 1.5 hours, with a cooling rate of 1.5°C / min, and then cool to 750°C at a rate of 1.5°C / min, and finally cool to room temperature with the furnace. In this step, during the process of cooling from 1200°C to 750°C (that is, when the temperature in the pouring chamber drops below 1200°C), the vacuum chamber can be connected to the atmosphere to allow the molten metal in the riser to flow back into the crucible.
[0091] The fourth step is to take out the casting after it cools down and cut off the pouring system part to obtain the alumina / iron composite casting.
[0092] Example 3
[0093] This embodiment provides a method for bonding iron-based metal and alumina ceramic based on binder injection molding technology, which specifically includes the following steps:
[0094] The first step is to manufacture the hollow ceramic shell by using a binder injection molding technology. Specifically, the preparation of the ceramic shell includes the following steps:
[0095] (1) Add 8 wt% of 1250 mesh MnO2 sintering aid to 1250 mesh alumina ceramic powder and mix for 4 hours using an automatic powder mixer;
[0096] (2) The ceramic shell is integrally formed by using a binder injection molding technology, and the blank is cured at 190°C for 2.5 hours. The binder used in the binder injection molding technology is a phenolic resin binder, and the detailed parameter conditions used in the injection molding are: the layer height is 0.1 mm, and the binder saturation is 120%.
[0097] (3) vacuum impregnating the solidified preform with a TiO2 sol having a solid content of 25% for 105 seconds at a vacuum degree of 25 KPa;
[0098] (4) drying the impregnated ceramic shell at 60° C. for 24 h until it is completely dehydrated;
[0099] (5) Degreasing and sintering the infiltrated and dried ceramic shell, the sintering parameters are set as follows: heating from room temperature to 660°C at a heating rate of 4°C / min, keeping the temperature for 90 min, then heating to 1050°C at a heating rate of 4°C / min, reducing the heating rate to 2°C / min to 1450°C, keeping the temperature for 3 h, and finally cooling to room temperature with the furnace;
[0100] The second step is to prepare the middle layer by vacuum dipping coating. The binder of the coating is silica sol with a solid content of 30%. The aggregate is titanium powder with a particle size of 1200 mesh and the aggregate accounts for 60wt%. The preparation process includes the following sub-steps:
[0101] (1) The coating was stirred at a speed of 2000 r / min for 15 min using a high-speed stirrer and then dip-coated. The dipping vacuum was 40 KPa and the dipping time was 40 s.
[0102] (2) After dip coating, the ceramic shell is placed in a vacuum reactor at a vacuum degree of 40 KPa for 2 h to ensure that the bubbles in the coating are completely precipitated;
[0103] (3) Drying the ceramic shell in a drying oven at 60° C. for 24 h;
[0104] (4) The process parameters for sintering the coating after drying are: heating from room temperature to 1300°C at a heating rate of 4°C / min, keeping the temperature for 60 min, and finally cooling to room temperature in the furnace. The resulting coating thickness is 240 μm.
[0105] The third step is to place the sintered coated ceramic shell in a vacuum chamber, preheat to 1200°C, keep warm for 45 minutes, use a negative pressure of -0.1MPa for vacuum casting, vacuum cast 65Mn spring steel liquid, pouring temperature 1650°C, keep the parts at 1400°C and 1200°C for 1.5 hours, the cooling rate in the middle is 1.5°C / min, and then cool to 750°C at a rate of 1.5°C / min, and finally cool to room temperature with the furnace. In this step, during the process of cooling from 1200°C to 750°C (that is, when the temperature in the pouring chamber drops below 1200°C), the vacuum chamber can be connected to the atmosphere to allow the molten metal in the riser to flow back into the crucible.
[0106] The fourth step is to take out the casting after it cools down and cut off the pouring system part to obtain the alumina / iron composite casting.
[0107] Example 4
[0108] This embodiment provides a method for bonding iron-based metal and alumina ceramic based on binder injection molding technology, which specifically includes the following steps:
[0109] The first step is to manufacture the hollow ceramic shell by using a binder injection molding technology. Specifically, the preparation of the ceramic shell includes the following steps:
[0110] (1) Add 10 wt% of 2000 mesh MnO2 sintering aid to 2000 mesh alumina ceramic powder and mix for 4 h using an automatic powder mixer;
[0111] (2) The ceramic shell is integrally formed by using a binder injection molding technology, and the blank is cured at 220°C for 3 hours. The binder used in the binder injection molding technology is a phenolic resin binder, and the detailed parameter conditions used in the injection molding are: the layer height is 0.05 mm, and the binder saturation is 140%.
[0112] (3) vacuum impregnating the solidified preform with a TiO2 sol having a solid content of 30% for 120 seconds at a vacuum degree of 30 KPa;
[0113] (4) drying the impregnated ceramic shell at 60° C. for 24 h until it is completely dehydrated;
[0114] (5) Degreasing and sintering the infiltrated and dried ceramic shell, the sintering parameters are set as follows: heating from room temperature to 660°C at a heating rate of 4°C / min, keeping the temperature for 90 min, then heating to 1050°C at a heating rate of 4°C / min, reducing the heating rate to 2°C / min to 1450°C, keeping the temperature for 4 h, and finally cooling to room temperature with the furnace;
[0115] The second step is to prepare the intermediate layer by chemical nickel plating, which includes the following sub-steps:
[0116] (1) The ceramic shell is placed in an ultrasonic cleaning machine and cleaned with anhydrous ethanol as a detergent for 20 minutes, and then replaced with deionized water and treated with ultrasound for 15 minutes to ensure that all stains that have penetrated into the pores of the ceramic are removed;
[0117] (2) placing the ceramic shell in a NaOH solution with a concentration of 700 g / L, roughening it at 50° C. for 45 min, and then ultrasonically cleaning it in deionized water for 30 min (i.e., each ultrasonic cleaning time is 30 min, repeated multiple times), and measuring the pH value of the solution after each cleaning until the pH drops to 7.5±0.1, ensuring that the roughening solution on the surface and in the ceramic pores is completely removed;
[0118] (3) Soaking the roughened ceramic shell in a sensitizing solution for 15 minutes for sensitization treatment. After sensitization, the ceramic shell needs to be rinsed under running deionized water for 25 seconds;
[0119] (4) The sensitized ceramic body needs to be immersed in the activation solution for 20 minutes for activation treatment. After immersion, the ceramic is rinsed with running deionized water for 25 seconds. In order to prevent the residual metal ions on the surface of the activated ceramic shell from contaminating the plating solution, the ceramic shell needs to be placed in a NaH2PO2 solution with a concentration of 24g / L and reduced for 5 minutes;
[0120] (5) Place the sensitized and cleaned ceramic shell into a prepared plating solution beaker, place the beaker into a constant temperature electric water bath and heat to 70°C for chemical plating, and stir the plating solution at a uniform speed for 30 minutes. The chemical nickel plating solution in this step is a mixed solution of NiSO4, NaH2PO2, C4H6O5 and C2H4NaO2, wherein the content of NiSO4 is 30g / L, the content of NaH2PO2 is 30g / L, the content of C4H6O5 is 10g / L and the content of C2H4NaO2 is 7.5g / L (of course, other common plating solutions for chemical nickel plating can also be used).
[0121] (6) After nickel plating, the ceramic is taken out and cleaned, and then the coating is kept at 220°C for 50 minutes in an electric constant temperature drying oven and cooled in the furnace. The thickness of the obtained intermediate layer is 10 μm.
[0122] The third step is to place the sintered coated ceramic shell in a vacuum chamber, preheat to 1200°C, keep warm for 60 minutes, use a negative pressure of -0.75MPa for vacuum casting, vacuum cast 65Mn spring steel liquid, and pour at 1600°C. After pouring, keep the parts at 1500°C, 1400°C, 1300°C and 1200°C for 2 hours, with a cooling rate of 2°C / min in the middle, and then cool to 800°C at a rate of 2°C / min, and finally cool to room temperature with the furnace. In this step, during the process of cooling from 1200°C to 800°C (that is, when the temperature in the pouring chamber drops below 1200°C), the vacuum chamber can be connected to the atmosphere to allow the molten metal in the riser to flow back into the crucible.
[0123] The fourth step is to take out the casting after it cools down and cut off the pouring system part to obtain the alumina / iron composite casting.
[0124] The above embodiments are only examples, for example, the process can be adjusted according to the thickness requirements of the intermediate layer. In addition to chemical nickel plating, other chemical plating processes known in the prior art can also be used to form an intermediate layer containing the target metal material (the target metal ions and their concentrations in the plating solution can also be adjusted according to actual needs).
[0125] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A ceramic / metal interface bonding method based on binder injection molding, characterized in that: The following steps are involved: S1 is based on 3D printing and designs a castable hollow ceramic shell according to the structure of the target casting; S2 uses binder injection molding technology to 3D print the hollow ceramic shell to obtain a blank, and then successively undergoes curing, vacuum infiltration, drying and degreasing sintering to obtain a ceramic shell; wherein the degreasing sintering is used to remove the binder by sintering; S3 deposits an intermediate layer containing a metal material on the inner surface of the ceramic shell by vacuum dipping or chemical plating; S4 uses a casting method to fill the iron-based metal liquid into the interior of a ceramic shell with an intermediate layer deposited thereon. After temperature-controlled solidification and heat preservation treatment, a casting with a ceramic / metal interface bond can be obtained after cooling.
2. The ceramic / metal interface bonding method based on binder injection molding as claimed in claim 1, characterized in that: Step S2 specifically comprises pre-mixing the ceramic powder to be printed with the sintering aid MnO2, and then 3D printing the obtained mixture using a binder injection molding technology to obtain a preform; wherein the mass proportion of the sintering aid MnO2 in the mixture is 6% to 10%, and the particle sizes of the sintering aid and the ceramic powder are both between 500 and 2000 meshes; preferably, the ceramic powder is alumina ceramic powder; In step S2, the curing temperature used for curing is 160-220°C and the curing time is 2-3h; The vacuum impregnation liquid used is TiO2 sol, with a solid content of 20-30wt%, an impregnation time of 90-120s, and an impregnation vacuum of 20-30KPa; The process parameters of the debinding sintering are: heating from room temperature to 640-660°C at a heating rate of 2-4°C / min, and keeping warm for 60-90 minutes; then heating to 950-1050°C at a heating rate of 2-4°C / min; then heating to 1400-1450°C at a heating rate of 1-2°C / min, and keeping warm for 2-4 hours; finally cooling to room temperature with the furnace.
3. The ceramic / metal interface bonding method based on binder injection molding as claimed in claim 1, characterized in that: Step S3 specifically uses a vacuum dip coating method, wherein the coating is a mixture of aggregate and a coating binder; wherein the coating binder is a silica sol with a solid content of 20-40wt%; the aggregate is a metal element powder with a particle size of 1000-1200 meshes, and the melting point of the metal element is 1400-1800°C; the mass percentage of the aggregate in the coating is 40-60%; preferably, the metal element powder is nickel powder, chromium powder or titanium powder; Step S3 specifically includes the following sub-steps: S3.1 Stir the coating with a high-speed mixer at a speed of 1500-2000 r / min for 10-15 min, and then perform vacuum dipping; the vacuum degree of vacuum dipping is 20-40 KPa, and the dipping time is 20-40 s; S3.2 Place the vacuum-coated ceramic shell in a vacuum environment with a vacuum degree of 20 to 40 KPa for 1 to 2 hours to completely precipitate the bubbles in the coating; S3.3 drying the ceramic shell obtained in step S3.2 at a temperature of 40 to 60° C. for 18 to 24 hours; S3.4 sintering the ceramic shell obtained in step S3.3 to sinter the coating; the process parameters of the sintering treatment are: heating from room temperature to 1200-1300°C at a heating rate of 2-4°C / min, keeping warm for 30-60 minutes, and finally cooling to room temperature with the furnace.
4. The ceramic / metal interface bonding method based on binder injection molding as claimed in claim 1, characterized in that: Step S3 specifically uses a chemical nickel plating method, and the corresponding intermediate layer obtained is a metal nickel layer; Step S3 specifically includes the following sub-steps: S3-1 Use anhydrous ethanol as a cleaning agent to ultrasonically clean the ceramic shell for 15 to 30 minutes, and then change to deionized water as a cleaning agent to ultrasonically clean the ceramic shell for 5 to 20 minutes to ensure that all stains that have penetrated into the ceramic pores are removed; S3-2: placing the ceramic shell treated in step S3-1 into a NaOH solution with a concentration of 500 to 800 g / L, roughening it at 40 to 60° C. for 30 to 60 min, and then ultrasonically cleaning it multiple times using deionized water as a detergent, each ultrasonic cleaning time being 20 to 40 min, and measuring the pH value of the solution after each cleaning until the pH drops to 7.4 to 7.6, ensuring that the roughening solution on the surface and in the ceramic pores is completely removed; S3-3: Soak the ceramic shell treated in step S3-2 in a sensitizing solution for 10 to 25 minutes for sensitization treatment, and then rinse the ceramic shell under running deionized water for 20 to 30 seconds after sensitization; S3-4: Soak the ceramic shell treated in step S3-3 in an activation solution for 15 to 25 minutes for activation treatment, and then rinse the ceramic shell under flowing deionized water for 20 to 30 seconds after activation; then, place the obtained ceramic shell in a NaH2PO2 solution with a concentration of 18 to 30 g / L and reduce it for 3 to 8 minutes; S3-5 placing the ceramic shell treated in step S3-4 in a plating solution and performing chemical plating at a temperature of 60 to 80° C.; during the chemical plating process, stirring the plating solution at a uniform speed, and the plating time is 20 to 40 minutes; After S3-6 nickel plating is completed, take out the ceramic shell, clean it, and keep it at 180-250℃ for 40-60min, and then cool it down with the furnace.
5. The ceramic / metal interface bonding method based on binder injection molding as claimed in claim 1, characterized in that: In step S4, the iron-based molten metal is 65Mn spring steel liquid; The casting is specifically gravity casting, and the pouring temperature used is 1600-1700° C.; or, the casting is specifically vacuum suction casting, and the pouring temperature used is 1550-1650° C., and the negative pressure used is -0.05--0.1 MPa.
6. The ceramic / metal interface bonding method based on binder injection molding as claimed in claim 1, characterized in that: In step S4, the ceramic shell is preheated at above 1200° C. for 30 to 60 minutes before being cast; The temperature-controlled solidification and heat preservation treatment is specifically to cool the workpiece at a preset rate after pouring is completed, and in the range of 1600-1200°C, keep the temperature for 1-2 hours after each 100°C-200°C reduction until the temperature drops to 700-800°C, and finally cool to room temperature with the furnace; the preset rate is specifically 1-2°C / min.
Citation Information
Patent Citations
Self-propagating high-temperature synthesis (SHS) process for preparing thick aluminium oxide ceramic coatings on steel plate surfaces
CN102978616A
Aluminum oxide ceramic surface metallization method
CN114988918A
Preparing method for casting inlaid ceramic / metal wear-resisting compound liner
CN106077582A
Preparation method of layered metal-ceramic composite material part
CN107353008A
Preparation method of surface-modified ZTA ceramic particle reinforced steel based composite material
CN109706438A