Polishing pad with uniform pores and preparation method thereof

By replacing the high-temperature expansion ball with p-toluenesulfonamide, fine and uniform pores are formed, which solves the problems of polishing uniformity and metal particles in traditional polyurethane polishing pads, and improves the pore uniformity and mass stability of the polishing pads.

CN118905914AActive Publication Date: 2024-11-08SHANGHAI XINQIAN INTEGRATED CIRCUIT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172356.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-08
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Traditional polyurethane polishing pads cannot meet the precision polishing requirements in terms of dynamic polishing uniformity, concave deformation and mechanical properties, resulting in high replacement frequency of polishing pads, affecting the polishing quality and efficiency, and micropores and metals caused by uneven dispersion of high-temperature expansion balls The residue of particles causes damage to the wafer.

Method used

P-toluenesulfonamide is used instead of high-temperature expansion balls. Through uniform mixing and inflating with polyurethane prepolymer and chain extender, fine and uniform pores are formed, reducing the density of the polishing pad, avoiding metal particles residues, and improving the mixing uniformity of raw materials.

Benefits of technology

The uniformity of pore distribution and mass stability of the polishing pad are achieved, the density of the polishing pad is reduced, the residue of metal particles is avoided, and the polishing performance and product uniformity are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905914A_ABST
    Figure CN118905914A_ABST
Patent Text Reader

Abstract

The invention relates to a polishing pad with uniform pores and a preparation method thereof, the preparation method comprises the following steps: (a) respectively weighing the following raw materials in parts by weight: 70-80 parts of a polyurethane prepolymer, 3-5 parts of a foaming agent and 15-24 parts of a chain extender, the foaming agent being p-toluene sulfonamide; (b) respectively softening the polyurethane prepolymer and the chain extender; (c) dissolving the blowing agent; (d) uniformly mixing the polyurethane prepolymer and the foaming agent to obtain a first mixture; (e) uniformly mixing the chain extender and the first mixture to obtain a second mixture; and (f) carrying out mold curing treatment on the second mixture. Compared with the prior art, the method has the advantages that high-temperature expansion balls are replaced with the p-toluene sulfonamide (TSH), the p-toluene sulfonamide can be heated to decompose nitrogen, closed, fine and uniform air holes are formed in the polishing pad, so that internal pore forming of the polishing pad is achieved, the density of the polishing pad is reduced, and metal particle residues caused by the high-temperature expansion balls are effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polishing pad preparation, in particular to a polishing pad with uniform pores and a preparation method thereof. Background Art

[0002] In the process of Chemical Mechanical Ploshing (CMP), the polishing pad plays the role of storing and transporting polishing liquid, discharging waste, transferring processing load, and ensuring the smoothness of the polishing process. The quality of the polishing pad directly affects the polishing effect. Improving the quality of the polishing pad is crucial to improving the quality of wafer manufacturing. Common CMP polishing pads include polyurethane polishing pads, non-woven polishing pads, and synthetic leather polishing pads. Among them, polyurethane has the highest polishing removal rate and is currently the most commonly used polishing pad material.

[0003] However, as precision electronic devices have increasingly higher requirements for the polishing precision of integrated circuits and chip surfaces, traditional polyurethane polishing pads cannot fully meet the requirements of precision polishing in terms of dynamic polishing uniformity, concave deformation, and mechanical properties, resulting in a high frequency of polishing pad replacement, affecting polishing quality and polishing efficiency.

[0004] In order to obtain a polyurethane polishing pad with more uniform pores, the existing polyurethane polishing pad is pre-mixed with a liquid polyurethane material through a PET high-temperature expansion ball, and then a certain amount of chain extender is added before curing and forming in a mold. The cured sample is subjected to multiple subsequent processing steps such as slicing, carving, and lamination to form the final polishing pad. However, the polyurethane polishing pad obtained by using the high-temperature expansion ball is prone to electrostatic agglomeration during the raw material mixing process, resulting in uneven dispersion of the high-temperature expansion ball, and finally forming micropores of different sizes inside the polishing pad, resulting in unstable quality of the polishing pad. At the same time, the metal particles in the high-temperature expansion ball will remain inside the polishing pad and be released during the polishing process, thereby causing irreversible damage to the wafer such as scratches or electrostatic breakdown. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a polishing pad with uniform pores and a preparation method thereof, so as to improve the uniformity of the pore distribution of the polishing pad.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A method for preparing a polishing pad with uniform pores comprises the following steps:

[0008] (a) Weighing the following raw materials by weight: 70-80 parts of a polyurethane prepolymer, 3-5 parts of a blowing agent, and 15-24 parts of a chain extender, wherein the blowing agent is p-toluenesulfonamide;

[0009] (b) softening the polyurethane prepolymer and the chain extender respectively;

[0010] (c) dissolving the blowing agent;

[0011] (d) uniformly mixing the polyurethane prepolymer and the blowing agent to obtain a first mixture;

[0012] (e) uniformly mixing the chain extender and the first mixture to obtain a second mixture;

[0013] (f) subjecting the second mixture to a mold curing process.

[0014] In one embodiment, in the step (c), the following steps are included: using anhydrous ethanol to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 5:1 to 10:1;

[0015] In the step (d), the following steps are included: fully stirring the mixed polyurethane prepolymer and the foaming agent; and subjecting the stirred polyurethane prepolymer and the foaming agent to a constant temperature baking treatment, the baking temperature being 70 to 80° C. and the baking time being 15 to 20 minutes, to obtain the first mixture.

[0016] In one embodiment, between step (d) and step (e), the following step is also included: aerating and mixing the first mixture, injecting nitrogen above the first mixture, the nitrogen pressure is 5 to 8 bar, the aerating and mixing temperature is 50 to 80° C., and the aerating and mixing time is 3 to 4 hours.

[0017] In one embodiment, in the step (b), the softening temperature of the polyurethane prepolymer is 50-70° C., and the softening time of the polyurethane prepolymer is 3-5 hours.

[0018] In one embodiment, in the step (b), the chain extender is 4,4'-methylenebis(2-chloroaniline), the softening temperature of the chain extender is 100-120°C, and the softening time of the chain extender is 4 hours.

[0019] In one embodiment, in the step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50-80° C., and the softening time of the chain extender is 4 hours.

[0020] In one embodiment, in step (a), the density of the polyurethane prepolymer is 1100-1190 Kg / m 3The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 70 to 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 6.5% to 11.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0021] In one embodiment, in step (a), the weight components of the raw materials are: 73-75 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 20-24 parts of chain extender.

[0022] In one embodiment, in the step (f), the following steps are included:

[0023] Preheating the mold, the mold preheating temperature is ≥110°C, and the mold preheating time is ≥5h;

[0024] pouring the second mixture into a preheated mold;

[0025] The mold is placed in a constant temperature oven for curing, the curing temperature is 110-120° C., and the curing time is ≥15 hours.

[0026] A polishing pad with uniform pores is prepared by using the above preparation method.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] 1. The above preparation method uses p-toluenesulfonamide (TSH) instead of high-temperature expansion balls. P-toluenesulfonamide will decompose nitrogen when heated to form closed, fine and uniform pores inside the polishing pad to achieve pore formation inside the polishing pad, thereby reducing the density of the polishing pad and effectively avoiding the metal particle residue caused by the high-temperature expansion balls. In the preparation process, the polyurethane prepolymer and the foaming agent are first mixed, and then the chain extender is mixed, which is conducive to the full and uniform distribution of the foaming agent in the mixture, so as to form pores with uniform density and pore size at each location of the polishing pad. At the same time, the polyurethane prepolymer and the chain extender are softened and then mixed, and the foaming agent is dissolved and then mixed, so as to further improve the uniformity of the raw material mixing, thereby improving the uniformity of the polishing pad product quality.

[0029] 2. As an organic solvent, anhydrous ethanol can dissolve p-toluenesulfonamide well, promote the uniform mixing of p-toluenesulfonamide into the polyurethane prepolymer, and can be removed from the raw material mixture by heating after uniform mixing, thereby avoiding the influence of the solvent on the quality of the polishing pad and helping to improve the production quality of the polishing pad.

[0030] 3. 4,4'-methylenebis(2-chloroaniline) (MOCA) and dimethylthiotoluenediamine (DMTDA) are both good and commonly used chain extenders. Therefore, selecting different softening temperatures and softening times according to different chain extenders is beneficial to improving the softening effect of the chain extender, thereby improving the uniformity of raw material mixing.

[0031] 4. When pouring and curing the raw material mixture, preheat the mold first to ensure that the temperature of the mold is close to the curing temperature and the temperature of the mold is uniform. This will avoid uneven heating of the raw material mixture after it is poured into the mold, and local rapid cooling and curing, which will lead to unstable quality of the polishing pad. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The process flow chart of the polishing pad preparation method of the present invention.

[0033] Figure 2 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 1.

[0034] Figure 3 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 2.

[0035] Figure 4 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 3.

[0036] Figure 5 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 4.

[0037] Figure 6 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 5.

[0038] Figure 7 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 6.

[0039] Figure 8 This is a scanning electron microscope (SEM) image of the polishing pad prepared in Example 7. DETAILED DESCRIPTION

[0040] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0041] A polishing pad with uniform pores and a preparation method thereof are described in detail below in conjunction with the accompanying drawings.

[0042] like Figure 1As shown, in one embodiment, a method for preparing a polishing pad with uniform pores is provided, comprising the following steps:

[0043] (a) Weighing the following raw materials by weight: 70-80 parts of a polyurethane prepolymer, 3-5 parts of a blowing agent, and 15-24 parts of a chain extender, wherein the blowing agent is p-toluenesulfonamide;

[0044] (b) softening the polyurethane prepolymer and the chain extender respectively;

[0045] (c) dissolving the blowing agent;

[0046] (d) uniformly mixing the polyurethane prepolymer and the blowing agent to obtain a first mixture;

[0047] (e) uniformly mixing the chain extender and the first mixture to obtain a second mixture;

[0048] (f) subjecting the second mixture to a mold curing process.

[0049] The above preparation method uses p-toluenesulfonamide (TSH) to replace the high-temperature expansion balls. P-toluenesulfonamide will decompose nitrogen when heated to form closed, fine and uniform pores inside the polishing pad to achieve pore formation inside the polishing pad, thereby reducing the density of the polishing pad and effectively avoiding the metal particle residue caused by the high-temperature expansion balls. In the preparation process, the polyurethane prepolymer and the foaming agent are first mixed, and then the chain extender is mixed, which is conducive to the full and uniform distribution of the foaming agent in the mixture, so as to form pores with uniform density and pore size at each location of the polishing pad. At the same time, the polyurethane prepolymer and the chain extender are softened and then mixed, and the foaming agent is dissolved and then mixed, so as to further improve the uniformity of the raw material mixing, thereby improving the uniformity of the polishing pad product quality.

[0050] Specifically, in one embodiment, in the step (c), the following steps are included: using anhydrous ethanol to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 5:1 to 10:1;

[0051] In the step (d), the following steps are included: fully stirring the mixed polyurethane prepolymer and the foaming agent; and subjecting the stirred polyurethane prepolymer and the foaming agent to a constant temperature baking treatment, the baking temperature being 70 to 80° C. and the baking time being 15 to 20 minutes, to obtain the first mixture.

[0052] Furthermore, in one of the embodiments, the ratio of the anhydrous ethanol to the foaming agent is 8:1; the baking temperature is 75° C., and the baking time is 20 min to obtain the first mixture.

[0053] As an organic solvent, anhydrous ethanol can dissolve p-toluenesulfonamide well, promote the uniform mixing of p-toluenesulfonamide into the polyurethane prepolymer, and can be removed from the raw material mixture by heating after uniform mixing, thereby avoiding the influence of the solvent on the quality of the polishing pad and helping to improve the production quality of the polishing pad.

[0054] Specifically, in one embodiment, between step (d) and step (e), the following step is also included: aerating and mixing the first mixture, injecting nitrogen above the first mixture, the nitrogen pressure is 5 to 8 bar, the aerating and mixing temperature is 50 to 80° C., and the aerating and mixing time is 3 to 4 hours.

[0055] Furthermore, the first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 50° C., and the aeration and mixing time is 4 hours.

[0056] Furthermore, the first mixture is aerated and mixed, nitrogen is filled above the first mixture, the nitrogen pressure is 8 bar, the aeration and mixing temperature is 80° C., and the aeration and mixing time is 3 hours.

[0057] Specifically, in one of the embodiments, in the step (b), the softening temperature of the polyurethane prepolymer is 50 to 70° C., and the softening time of the polyurethane prepolymer is 3 to 5 hours.

[0058] Furthermore, in the step (b), the softening temperature of the polyurethane prepolymer is 50° C., and the softening time of the polyurethane prepolymer is 5 hours.

[0059] Furthermore, in the step (b), the softening temperature of the polyurethane prepolymer is 70° C., and the softening time of the polyurethane prepolymer is 3 hours.

[0060] Furthermore, in the step (b), the softening temperature of the polyurethane prepolymer is 60° C., and the softening time of the polyurethane prepolymer is 4 hours.

[0061] Specifically, in one embodiment, in the step (b), the chain extender is 4,4'-methylenebis(2-chloroaniline), the softening temperature of the chain extender is 100-120°C, and the softening time of the chain extender is 4h.

[0062] Furthermore, in one of the embodiments, in the step (b), the chain extender is 4,4'-methylenebis(2-chloroaniline), the softening temperature of the chain extender is 100°C, and the softening time of the chain extender is 4h.

[0063] Furthermore, in one of the embodiments, in the step (b), the chain extender is 4,4'-methylenebis(2-chloroaniline), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4h.

[0064] Furthermore, in one of the embodiments, in the step (b), the chain extender is 4,4'-methylenebis(2-chloroaniline), the softening temperature of the chain extender is 120°C, and the softening time of the chain extender is 4h.

[0065] Specifically, in one embodiment, in the step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50-80° C., and the softening time of the chain extender is 4 hours.

[0066] Furthermore, in one of the embodiments, in the step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 70° C., and the softening time of the chain extender is 4 hours.

[0067] Furthermore, in one of the embodiments, in the step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 50° C., and the softening time of the chain extender is 4 hours.

[0068] Furthermore, in one of the embodiments, in the step (b), the chain extender is dimethylthiotoluene diamine, the softening temperature of the chain extender is 80° C., and the softening time of the chain extender is 4 hours.

[0069] 4,4'-methylenebis(2-chloroaniline) (MOCA) and dimethylthiotoluenediamine (DMTDA) are both good and commonly used chain extenders. Therefore, selecting different softening temperatures and softening times according to different chain extenders is beneficial to improving the softening effect of the chain extender, thereby improving the uniformity of raw material mixing.

[0070] Specifically, in one embodiment, in the step (a), the density of the polyurethane prepolymer is 1100-1190 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 70 to 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 6.5% to 11.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0071] Furthermore, in one embodiment, in the step (a), the density of the polyurethane prepolymer is 1100 Kg / m 3The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 100 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 7.5%, and the moisture content in the polyurethane prepolymer is 400 ppm.

[0072] Specifically, in one of the embodiments, in step (a), the weight components of the raw materials are: 73-75 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 20-24 parts of chain extender.

[0073] Furthermore, in one of the embodiments, in the step (a), the weight components of the raw materials are: 75 parts of polyurethane prepolymer, 4 parts of foaming agent and 22 parts of chain extender.

[0074] Furthermore, in one of the embodiments, in the step (a), the weight components of the raw materials are: 73 parts of polyurethane prepolymer, 3 parts of foaming agent and 20 parts of chain extender.

[0075] Furthermore, in one of the embodiments, in the step (a), the weight components of the raw materials are: 74 parts of polyurethane prepolymer, 5 parts of foaming agent and 24 parts of chain extender.

[0076] Specifically, in one embodiment, in the step (f), the following steps are included:

[0077] Preheating the mold, the mold preheating temperature is ≥110°C, and the mold preheating time is ≥5h;

[0078] pouring the second mixture into a preheated mold;

[0079] The mold is placed in a constant temperature oven for curing, the curing temperature is 110-120° C., and the curing time is ≥15 hours.

[0080] Furthermore, in one of the embodiments, in the step (f), the mold preheating temperature is ≥115°C, the mold preheating time is 6 hours, the curing temperature is 115°C, and the curing time is 17 hours.

[0081] When pouring and curing the raw material mixture, preheat the mold first to ensure that the temperature of the mold is close to the curing temperature and the temperature of the mold is uniform. This will avoid uneven heating of the raw material mixture after it is poured into the mold, and local rapid cooling and curing, which will lead to unstable quality of the polishing pad.

[0082] In one embodiment, a polishing pad with uniform pores is provided, which is prepared by the above-mentioned preparation method.

[0083] The above preparation method uses p-toluenesulfonamide (TSH) to replace the high-temperature expansion balls. P-toluenesulfonamide will decompose nitrogen when heated to form closed, fine and uniform pores inside the polishing pad to achieve pore formation inside the polishing pad, thereby reducing the density of the polishing pad and effectively avoiding the metal particle residue caused by the high-temperature expansion balls. In the preparation process, the polyurethane prepolymer and the foaming agent are first mixed, and then the chain extender is mixed, which is conducive to the full and uniform distribution of the foaming agent in the mixture, so as to form pores with uniform density and pore size at each location of the polishing pad. At the same time, the polyurethane prepolymer and the chain extender are softened and then mixed, and the foaming agent is dissolved and then mixed, so as to further improve the uniformity of the raw material mixing, thereby improving the uniformity of the polishing pad product quality.

[0084] Example 1

[0085] The polishing pad obtained by the preparation method of Example 1 is as follows Figure 2 As shown, the specific steps are as follows:

[0086] Weigh the following raw materials by weight: 75 parts of polyurethane prepolymer, 4 parts of high temperature expansion ball and 20 parts of chain extender. The density of the polyurethane prepolymer is 1100 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 10.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0087] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60° C., and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is 4,4'-methylenebis-(2-chloroaniline) (MOCA), and the softening temperature of the chain extender is 110° C., and the softening time of the chain extender is 4 hours.

[0088] The polyurethane prepolymer and the high-temperature expansion ball are fully stirred and mixed; the stirred polyurethane prepolymer and the high-temperature expansion ball are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0089] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0090] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0091] pouring the second mixture into a preheated mold;

[0092] The mold was placed in a constant temperature oven for curing, the curing temperature was 120° C., and the curing time was 16 hours.

[0093] Example 2

[0094] Example 2 Compared with Example 1, p-toluenesulfonamide foaming agent is used to replace high temperature expansion balls to prepare the polishing pad, and other components and process conditions remain unchanged. The polishing pad obtained by the preparation method of Example 2 is as follows Figure 3 As shown, the specific steps are as follows:

[0095] The following raw materials were weighed respectively: 75 parts of polyurethane prepolymer, 4 parts of foaming agent and 20 parts of chain extender, wherein the foaming agent was p-toluenesulfonamide, and the density of the polyurethane prepolymer was 1100 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 10.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0096] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60° C., and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is 4,4'-methylenebis-(2-chloroaniline) (MOCA), and the softening temperature of the chain extender is 110° C., and the softening time of the chain extender is 4 hours.

[0097] Anhydrous ethanol is used to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 8:1.

[0098] The polyurethane prepolymer and the foaming agent are fully stirred and mixed; the stirred polyurethane prepolymer and the foaming agent are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0099] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0100] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0101] pouring the second mixture into a preheated mold;

[0102] The mold was placed in a constant temperature oven for curing, the curing temperature was 120° C., and the curing time was 16 hours.

[0103] Example 3

[0104] Example 3 Compared with Example 2, the raw material ratio is changed, and other components and process conditions remain unchanged. The polishing pad obtained by the preparation method of Example 3 is as follows: Figure 4 As shown, the specific steps are as follows:

[0105] The following raw materials were weighed by weight: 100 parts of polyurethane prepolymer, 2 parts of foaming agent and 22 parts of chain extender, wherein the foaming agent was p-toluenesulfonamide and the density of the polyurethane prepolymer was 1100 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 8.5%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0106] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60° C., and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is 4,4'-methylenebis-(2-chloroaniline) (MOCA), and the softening temperature of the chain extender is 110° C., and the softening time of the chain extender is 4 hours.

[0107] Anhydrous ethanol is used to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 8:1.

[0108] The polyurethane prepolymer and the foaming agent are fully stirred and mixed; the stirred polyurethane prepolymer and the foaming agent are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0109] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0110] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0111] pouring the second mixture into a preheated mold;

[0112] The mold was placed in a constant temperature oven for curing, the curing temperature was 120° C., and the curing time was 16 hours.

[0113] Example 4

[0114] Example 4 Compared with Example 2, the raw material ratio is changed, and other components and process conditions remain unchanged. The polishing pad obtained by the preparation method of Example 4 is as follows: Figure 5 As shown, the specific steps are as follows:

[0115] The following raw materials were weighed by weight: 100 parts of polyurethane prepolymer, 0.5 parts of foaming agent and 24 parts of chain extender, wherein the foaming agent was p-toluenesulfonamide, and the density of the polyurethane prepolymer was 1100 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 9.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0116] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60° C., and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is 4,4'-methylenebis-(2-chloroaniline) (MOCA), and the softening temperature of the chain extender is 110° C., and the softening time of the chain extender is 4 hours.

[0117] Anhydrous ethanol is used to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 8:1.

[0118] The polyurethane prepolymer and the foaming agent are fully stirred and mixed; the stirred polyurethane prepolymer and the foaming agent are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0119] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0120] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0121] pouring the second mixture into a preheated mold;

[0122] The mold was placed in a constant temperature oven for curing, the curing temperature was 120° C., and the curing time was 16 hours.

[0123] Example 5

[0124] Example 5 Compared with Example 2, DMTDA (dimethylthiotoluenediamine) is used as a chain extender, and the raw material ratio, curing temperature and time are changed, while other components and process conditions remain unchanged. The polishing pad obtained by the preparation method of Example 5 is as follows Figure 6 As shown, the specific steps are as follows:

[0125] The following raw materials were weighed by weight: 100 parts of polyurethane prepolymer, 4 parts of foaming agent and 20 parts of chain extender, wherein the foaming agent was p-toluenesulfonamide, and the density of the polyurethane prepolymer was 1100 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 10.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0126] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60°C, and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is DMTDA (dimethylthiotoluenediamine), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4 hours.

[0127] Anhydrous ethanol is used to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 8:1.

[0128] The polyurethane prepolymer and the foaming agent are fully stirred and mixed; the stirred polyurethane prepolymer and the foaming agent are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0129] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0130] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0131] pouring the second mixture into a preheated mold;

[0132] The mold was placed in a constant temperature oven for curing, the curing temperature was 110° C., and the curing time was 20 hours.

[0133] Example 6

[0134] Example 6 Compared with Example 2, DMTDA (dimethylthiotoluenediamine) is used as a chain extender, and the raw material ratio, curing temperature and time are changed, while other components and process conditions remain unchanged. The polishing pad obtained by the preparation method of Example 6 is as follows: Figure 7 As shown, the specific steps are as follows:

[0135] The following raw materials were weighed by weight: 100 parts of polyurethane prepolymer, 2 parts of foaming agent and 22 parts of chain extender, wherein the foaming agent was p-toluenesulfonamide and the density of the polyurethane prepolymer was 1100 Kg / m 3The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 10.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0136] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60°C, and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is DMTDA (dimethylthiotoluenediamine), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4 hours.

[0137] Anhydrous ethanol is used to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 8:1.

[0138] The polyurethane prepolymer and the foaming agent are fully stirred and mixed; the stirred polyurethane prepolymer and the foaming agent are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0139] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0140] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0141] pouring the second mixture into a preheated mold;

[0142] The mold was placed in a constant temperature oven for curing, the curing temperature was 110° C., and the curing time was 20 hours.

[0143] Example 7

[0144] Example 7 Compared with Example 2, DMTDA (dimethylthiotoluenediamine) is used as a chain extender, and the raw material ratio, curing temperature and time are changed, while other components and process conditions remain unchanged. The polishing pad obtained by the preparation method of Example 7 is as follows: Figure 8 As shown, the specific steps are as follows:

[0145] The following raw materials were weighed by weight: 100 parts of polyurethane prepolymer, 4 parts of foaming agent and 24 parts of chain extender, wherein the foaming agent was p-toluenesulfonamide, and the density of the polyurethane prepolymer was 1100 Kg / m 3The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 10.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

[0146] The polyurethane prepolymer and the chain extender are softened separately, the softening temperature of the polyurethane prepolymer is 60°C, and the softening time of the polyurethane prepolymer is 4 hours. The chain extender is DMTDA (dimethylthiotoluenediamine), the softening temperature of the chain extender is 110°C, and the softening time of the chain extender is 4 hours.

[0147] Anhydrous ethanol is used to dissolve the foaming agent, and the ratio of the anhydrous ethanol to the foaming agent is 8:1.

[0148] The polyurethane prepolymer and the foaming agent are fully stirred and mixed; the stirred polyurethane prepolymer and the foaming agent are subjected to a constant temperature baking treatment, the baking temperature is 75° C., and the baking time is 20 minutes, to obtain the first mixture.

[0149] The first mixture is aerated and mixed, and nitrogen is filled above the first mixture. The nitrogen pressure is 5 bar, the aeration and mixing temperature is 70° C., and the aeration and mixing time is 3 hours.

[0150] Preheating the mold, the mold preheating temperature is 115°C, and the mold preheating time is 6 hours;

[0151] pouring the second mixture into a preheated mold;

[0152] The mold was placed in a constant temperature oven for curing, the curing temperature was 110° C., and the curing time was 20 hours.

[0153] The polishing pad prepared in Example 1 is as follows Figure 2 As shown, the polishing pads prepared in Examples 2-7 are as follows Figure 3-8 As shown, it can be seen from the scanning electron microscope image of the polishing pad that the polishing pad prepared in Examples 2-7 has obviously more uniform pore distribution and smaller pore diameter. Therefore, the polishing pad prepared with p-toluenesulfonamide (TSH) has better polishing performance and effectively improves the pore uniformity and quality uniformity of the polishing pad.

[0154] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a polishing pad with uniform pores, characterized in that: The steps include: (a) Weighing the following raw materials by weight: 70-80 parts of a polyurethane prepolymer, 3-5 parts of a blowing agent, and 15-24 parts of a chain extender, wherein the blowing agent is p-toluenesulfonamide; (b) softening the polyurethane prepolymer and the chain extender respectively; (c) dissolving the foaming agent; (d) uniformly mixing the polyurethane prepolymer and the blowing agent to obtain a first mixture; (e) uniformly mixing the chain extender and the first mixture to obtain a second mixture; (f) performing a mold curing process on the second mixture.

2. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (c), the following steps are included: dissolving the foaming agent in anhydrous ethanol, wherein the ratio of the anhydrous ethanol to the foaming agent is 5:1 to 10:1; In the step (d), the following steps are included: fully stirring the mixed polyurethane prepolymer and the foaming agent; and performing a constant temperature baking treatment on the stirred polyurethane prepolymer and the foaming agent, the baking temperature being 70 to 80° C. and the baking time being 15 to 20 minutes to obtain the first mixture.

3. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: Between step (d) and step (e), the following step is also included: aerating and mixing the first mixture, injecting nitrogen above the first mixture, the nitrogen pressure is 5 to 8 bar, the aerating and mixing temperature is 50 to 80° C., and the aerating and mixing time is 3 to 4 hours.

4. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (b), the softening temperature of the polyurethane prepolymer is 50 to 70° C., and the softening time of the polyurethane prepolymer is 3 to 5 hours.

5. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (b), the chain extender is 4,4'-methylenebis-(2-chloroaniline), the softening temperature of the chain extender is 100-120°C, and the softening time of the chain extender is 4 hours.

6. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (b), the chain extender is dimethylthiotoluenediamine, the softening temperature of the chain extender is 50-80° C., and the softening time of the chain extender is 4 hours.

7. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (a), the density of the polyurethane prepolymer is 1100-1190 Kg / m 3 The Brookfield viscosity (30° C.) of the polyurethane prepolymer is 70 to 150 poise, the mass percentage of isocyanate groups (NCO) in the polyurethane prepolymer is 6.5% to 11.8%, and the moisture content in the polyurethane prepolymer is less than or equal to 500 ppm.

8. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (a), the weight components of the raw materials are: 73-75 parts of polyurethane prepolymer, 3-5 parts of foaming agent and 20-24 parts of chain extender.

9. The method for preparing a polishing pad with uniform pores according to claim 1, wherein: In the step (f), the following steps are included: Preheating the mold, the mold preheating temperature is ≥110°C, and the mold preheating time is ≥5h; pouring the second mixture into a preheated mold; The mold is placed in a constant temperature oven for curing, the curing temperature is 110-120° C., and the curing time is ≥15 h.

10. A polishing pad with uniform pores, characterized in that: The preparation method is described in any one of claims 1 to 9.