High-melting-point LCP film and manufacturing method and application thereof
Through the compressed aluminum clad method and step-process heating heat treatment, the problems of high dielectric loss and low peeling force in high-frequency communication were solved, and a high melting point film was prepared, which was suitable for the production of multi-layer boards and military applications, realizing the Efficient heat resistance and dimensional stability.
Patent Information
- Application Number
- CN202410947917.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing LCP film has high dielectric loss in high-frequency communications, and the traditional heating method leads to changes in surface morphology and low peeling force, making it unable to be used for the production of multi-layer boards, which limits its application in the military industry.
The LCP film is hot-pressed and bonded with aluminum foil by press-covered aluminum film, and the melting point is increased through step-by-step heat treatment to ensure the high heat resistance and peeling force of the film, which is suitable for the production of multi-layer boards.
It has achieved the preparation of high melting point LCP films, high peeling force, and is suitable for high-frequency communication substrates and military millimeter-wave radars and other fields. The products have excellent dimensional stability and heat resistance.
Smart Images

Figure CN118906507A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of LCP film processing, and in particular to a high melting point LCP film and a manufacturing method and application thereof. Background Art
[0002] High-frequency and high-speed communication is a new generation of high-frequency broadband mobile communication technology with the characteristics of high speed, low latency and large connection. In order to ensure the reliability of high-frequency and high-speed communication and reduce the loss of signals during transmission, high-frequency and high-speed substrates must use thin-film dielectric base materials with low dielectric constant (Dk) and low dielectric loss tangent (Df), and Dk and Df change little with temperature and frequency. The dielectric loss of traditional PI / MPI films is relatively high at high frequencies, especially when the signal transmission frequency exceeds 10GHz, this performance defect is amplified and cannot meet the requirements of antenna materials in the era of high-frequency communication. Compared with PI / MPI, LCP film has another important indicator, in addition to its low Df, which is its extremely low water absorption rate. Therefore, the loss-frequency curve of its substrate does not migrate significantly before and after moisture absorption. As a key material for high-frequency and high-speed signal transmission systems in electronic equipment, the successful development of LCP film's multi-layer flexible microwave composite dielectric substrate will directly support a new generation of electronic reconnaissance systems, such as radio frequency identification and positioning tracking. At the same time, the multilayer flexible composite dielectric substrate is a common material used in microwave components, and its expected application areas include airborne, missile-borne, satellite-borne and other platforms.
[0003] In order to ensure the product reliability of FCCL & FPC and meet military needs, higher requirements are also put forward for the heat resistance of LCP film. Generally speaking, resins with high melting points are more rigid and have lower melt strength, which cannot be directly obtained by known film making methods such as blow molding or biaxial stretching. Multi-stage heat treatment is usually used to increase the melting point of low-melting point films to improve the heat resistance of the films. Chinese patent CN 1232860A (authorization announcement number CN1206317C) discloses a method of attaching LCP film to metal foil and increasing the melting point through multi-stage temperature increase, wherein the first stage heat treatment temperature is Tdef~Tm-α (Tdef is the thermal deformation temperature of the film, Tm is the melting point of the film, α is 10~35°C), and the melting point is increased to TA1 after heat treatment. The second stage heat treatment temperature is Tm~TA1, and the melting point of the film is increased by analogy. However, this method is too close to the melting point in the later heat treatment. The surface of the film that is not bonded to the metal foil after the heat treatment cannot maintain its original morphology due to the intensified movement of the molecular segments. There is a risk of low peeling force after subsequent lamination with the copper foil. Therefore, it can only be used to produce single-sided boards, but cannot be used in the production of multi-layer boards, which limits its application in the military field. Japanese patents JP2010103269A and JP 2006179609A propose surface treatment of the film, and the treatment methods include physical grinding, liquid corrosion and ultraviolet treatment. However, physical grinding is prone to dust generation, and liquid corrosion is prone to residual liquid, which increases the process of the later treatment. In addition, the efficiency of ultraviolet treatment is low, which is not suitable for coil preparation. Summary of the invention
[0004] The primary purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and to provide a method for manufacturing a high melting point LCP film.
[0005] Another object of the present invention is to provide a high melting point LCP film manufactured by the method.
[0006] Another object of the present invention is to provide applications of the high melting point LCP film.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] A method for manufacturing a high melting point LCP film comprises the following steps:
[0009] (1) Pressing aluminum: The LCP film is hot-pressed with two layers of aluminum foil with a roughness of 1.5 μm to 2 μm (the LCP film is placed in the middle layer) to form an aluminum foil-LCP film-aluminum foil laminate; wherein the hot-pressing temperature is 10 to 30°C below the melting point of the LCP film, the pressure is 0.5 to 1.5 tons, and the speed is 0.5 to 1.5 m / min;
[0010] (2) Step-by-step temperature increase to improve melting point:
[0011] ① After peeling off one layer of the aluminum foil of the aluminum foil-LCP film-aluminum foil laminate obtained in step (1) using a slitting machine, loosen the LCP film coil using a film tensioning and winding machine, and then place the obtained sample in a high-temperature oxygen-free oven, bake it in the temperature range of the low-temperature inflection point Td1 to the high-temperature inflection point Td2 (Td1-Td2) of the LCP film for 4-6 hours to perform the first stage of melting point increase, and then perform the first sampling and measure the melting point, low-temperature inflection point Td1′ and high-temperature inflection point Td2′ of the sample; if the melting point is increased to above 330°C (preferably 330-340°C), then stop here and obtain the high melting point LCP film; if the melting point is lower than 330°C, proceed to the next step;
[0012] ② The remaining samples after the first sampling are further heated to Td1′~Td2′ and heat treated for 2~6h to increase the melting point in the second stage, and then the second sampling is performed to measure the melting point, low temperature inflection point Td1″ and high temperature inflection point Td2″ of the samples; if the melting point is increased to above 330°C (preferably 330~340°C), the high melting point LCP film is obtained; if the melting point is lower than 330°C, the next step is performed;
[0013] ③ Repeat step ② until the melting point is raised to above 330°C (preferably 330-340°C); after the heat treatment is completed, cool to 150°C, take out the film, and use a film tensioning machine to tighten the film, and then use a slitting machine to peel off the other layer of aluminum foil to obtain the high melting point LCP film.
[0014] The pressed aluminum coating in step (1) is performed by a roller press or a steel belt press; preferably, the aluminum coating is performed by a roller press.
[0015] The LCP film described in step (1) is a liquid crystal polyester; preferably a TLCP film; further preferably a film with a thickness of 25 to 100 μm, a melting point of 280 to 310°C, Td1 of 240 to 265°C, and Td2 of 260 to 288°C; further preferably an LCP film produced by Zhuhai Wantong Special Engineering Plastics Co., Ltd., with the grades ViFLEX-L and ViFLEX-M; wherein ViFLEX-L has a thickness of 50 μm, a melting point of 280°C, Td1 of 240°C, and Td2 of 260°C; and ViFLEX-M has a thickness of 50 μm, a melting point of 310°C, Td1 of 265°C, and Td2 of 288°C.
[0016] The aluminum foils described in step (1) have all been coated with a release agent.
[0017] The release agent is preferably a silicone release agent; further, it can be Ken-Tian Lusin Lub O 32F.
[0018] The aluminum foil described in step (1) is preferably aluminum foil 8021, and its bonding surface roughness Rz is 1.8 μm.
[0019] In step (1), the pressure of the hot pressing bonding is preferably 1 to 1.5 tons.
[0020] In step (1), the temperature of hot pressing bonding is 10 to 30°C below the melting point of the LCP film; preferably, it is 20 to 30°C below the melting point of the LCP film; for example, when the melting point of the selected raw material LCP film is 280°C, the temperature of hot pressing bonding is 250 to 270°C (preferably 250 to 260°C); for example, when the melting point of the selected raw material LCP film is 310°C, the temperature of hot pressing bonding is 280 to 300°C.
[0021] The speed of the hot pressing bonding in step (1) is preferably 1 m / min.
[0022] In step (2), during the heat treatment, the LCP film coil is placed vertically and nitrogen is circulated and purged in the vertical direction.
[0023] In step (2), the heating rate for increasing the melting point is preferably 5°C / min.
[0024] In step (2), the heat treatment temperature of each stage is between the low-temperature inflection point and the high-temperature inflection point (Td1~Td2, Td1′~Td2′, Td1″~Td2″) of the LCP film, wherein the low-temperature inflection point and the high-temperature inflection point are measured by rotational rheology. When the sample is heated to the melting point of the sample at 5°C / min, its storage modulus versus temperature curve has two inflection points, which are recorded as the low-temperature inflection point and the high-temperature inflection point from low to high temperatures, respectively.
[0025] In step (2), when the first stage of melting point increase is carried out, Td1 and Td2 are determined according to the raw material LCP film, that is, the treatment temperature for melting point increase is Td1~Td2 (preferably (Td1+10°C)~Td2), and the melting point of the LCP film is increased by 14~25°C (preferably 16~23°C); for example, when Td1 is 240°C and Td2 is 260°C, the temperature range of Td1~Td2 is 240°C~260°C (preferably 250~260°C).
[0026] In step (2), when the second stage of melting point increase is carried out, Td1′ and Td2′ are determined based on the LCP film sample after the melting point increase in the first stage, that is, the treatment temperature for melting point increase is Td1′~Td2′ (preferably (Td1′+10°C)~Td2′), and the melting point of the LCP film is increased by 25~40°C (preferably 26~39°C) relative to the raw material; for example, when Td1′ is 261~265°C and Td2′ is 279~284°C, the temperature range of Td1′~Td2′ is 261~284°C (preferably 275~280°C); for example, when Td1′ is 292°C and Td2′ is 331°C, the temperature range of Td1′~Td2′ is 292~311°C (preferably 302~311°C), and the same applies to others.
[0027] The cooling rate in step (2) is preferably below 10°C / min.
[0028] A high melting point TLCP film LCP film is manufactured by any of the methods described above.
[0029] The melting point of the high melting point LCP film is 330°C to 340°C, preferably 332°C to 336°C.
[0030] The high melting point LCP film is used in the fields of high-frequency and high-speed communication substrates, millimeter wave radars, airborne, missile-borne or satellite-borne equipment, etc.
[0031] The high-frequency and high-speed communication substrate includes a flexible copper clad laminate (Flexible Copper Clad Laminater, FCCL) and / or a flexible printed circuit (Flexible Printed Circuit, FPC).
[0032] The millimeter wave radar includes a military millimeter wave radar.
[0033] A flexible copper clad laminate (FCCL) comprises the above-mentioned high melting point LCP film and electrolytic copper foil.
[0034] The thickness of the electrolytic copper foil is preferably 12 to 18 μm.
[0035] The preparation method of the flexible copper clad laminate (FCCL) comprises the following steps: hot pressing the high melting point LCP film and the electrolytic copper foil to copper-clad both sides, the hot pressing temperature is 340-345°C, the pressure is 2-4MPa, and the hot pressing time is 5-10min.
[0036] The conditions for hot pressing double-sided copper cladding are preferably: hot pressing temperature 340° C., pressure 3 MPa, and time 6 min.
[0037] The present invention has the following beneficial effects compared with the prior art:
[0038] (1) The present invention provides a method for manufacturing a high-heat-resistant, high-melting-point LCP film, the manufacturing process of which is as follows: laminating the LCP film with a double-layer release aluminum foil to form an Al-LCP-Al laminate, then peeling off one layer of the aluminum foil, and performing a multi-stage programmed temperature rise heat treatment to achieve the effect of increasing the melting point. The high-melting-point film manufactured by this method has high peeling force, small difference in peeling force between the two sides, and a simple manufacturing method, which can directly produce a coil product, has high production efficiency, and small difference in melting point between different regions of the film coil.
[0039] (2) In the present invention, the surface morphology of the LCP film is given by the aluminum foil, so there are certain requirements for the roughness of the aluminum foil. If the roughness is too low, the effect of roughening the film cannot be achieved, while if the roughness is too high, aluminum powder is likely to fall off, affecting the electrical properties of the film.
[0040] (3) In the present invention, during heat treatment, the film coil is placed vertically, and nitrogen is circulated and purged in a vertical direction. At the same time, to ensure that the surface of the LCP film exposed to nitrogen during the heat treatment can still maintain its morphology, each heat treatment temperature can both ensure the movement of the film's molecular segments and prevent the film from slipping during the heat treatment. In order to ensure the efficiency of the film heat treatment, the present invention uses a high-temperature oxygen-free oven to heat the coil. During the heat treatment, the film undergoes solid-phase polycondensation and small molecule devolatilization. At the same time, in order to ensure that the inside and outside of the film are heated uniformly, the film needs to be loosened by a film tensioner before heat treatment. There is a certain distance between the coil layers to ensure that hot nitrogen flows on the film surface. After heat treatment, the film is tightened by a tensioner.
[0041] (4) The high melting point LCP film manufactured by the method of the present invention has a small difference in melting points at different parts of the coil, high double-sided peeling force after copper coating, small difference in double-sided peeling force, good heat resistance, and after slow cooling, the stress in the film is fully released, and the product has excellent dimensional stability.
[0042] (5) In the present invention, the LCP film is prepared by film blowing and post-processing of a composition containing a thermoplastic liquid crystal polymer, and the high melting point LCP film is prepared by raising the melting point of the low melting point LCP film by step-by-step temperature increase, and the melting point is between 330°C and 340°C.
[0043] (6) The high melting point LCP film prepared by the present invention through the optimization of aluminum foil and heat treatment process can be used to prepare FCCL and FPC, and can be applied to military millimeter wave radar, airborne, missile-borne, satellite-borne and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a schematic diagram of the film placement method and nitrogen purge direction.
[0045] Figure 2 This is a schematic diagram of the sampling positions for the melting point uniformity test (①-⑨ in the figure represent the sampling positions).
[0046] Figure 3 This is the rheological curve of ViFLEX-L. DETAILED DESCRIPTION
[0047] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the methods and equipment used in the present invention are conventional methods and equipment in the art. The test methods in the following examples where specific experimental conditions are not specified are usually based on conventional experimental conditions. Unless otherwise specified, the materials used in the present invention can be obtained commercially.
[0048] 1. The present invention uses the following method to evaluate the performance of the thermoplastic liquid crystal polymer:
[0049] 1. Melting point: measured by DSC 200F3 differential calorimeter manufactured by NETZSCH Company, with a heating rate of 20°C / min, from room temperature to 360°C above the melting point, then cooled to room temperature at 20°C / min, and finally heated to 30°C above the melting point at 20°C / min; the highest point of the melting peak of the first heating curve is taken as the melting point, and the lowest point of the crystallization peak of the first cooling curve is taken as the crystallization temperature.
[0050] 2. Melting point distribution uniformity: Take three points from the outside, middle and inside of the film roll along the TD direction (TD = transverse direction, i.e. perpendicular to the machine direction) and test the melting point of the sample according to the above method ( Figure 2 ), and then calculate the standard deviation of the nine points, which is the uniformity of the melting point distribution.
[0051] 3. Heat shock resistance: Referring to the standard GB / T 13557-2017, 8.2, after hot pressing the LCP film and copper foil, immerse it in a 288°C solder bath, maintain it for 10 seconds, take it out, and cool it down; after repeating it three times, observe whether the sample has blistering, stratification, etc.
[0052] 4. Copper coating peeling force: Cut a 10×160mm rectangular strip along the MD direction of the film (MD=machine direction, i.e., mechanical stretching direction or longitudinal direction), then peel it at 90° at a peeling speed of 50mm / min, and measure the peeling force (unit: N / mm) of the two sides respectively.
[0053] 5. Dimensional stability: Refer to GB / T 13557-2017, 7.1 test to measure the dimensional stability of the film after etching.
[0054] 6. Low temperature inflection point and high temperature inflection point test: Use The test method frequency is 10Hz, the test temperature range is Tm+30℃~230℃, where Tm is the melting point of the sample (the sample is heated to the melting point at 5℃ / min); the cooling rate is 10℃ / min, and the strain is 0.5%. The storage modulus versus temperature curve is obtained, and the curve is differentiated. The two temperature points where the slope begins to change suddenly are recorded as Td1 and Td2, Td1′ and Td2′, Td1″ and Td2″ from low to high.
[0055] 7. Dielectric loss: tested by SPDR resonant cavity method, test frequency 2.5GHz.
[0056] The above tests were repeated three times to take the average value.
[0057] 2. The material information used in the examples and comparative examples of the present invention is as follows:
[0058] 1. ViFLEX-L film:
[0059] The low melting point LCP film was purchased from Zhuhai Wantong Special Engineering Plastics Co., Ltd., with the brand names ViFLEX-L and ViFLEX-M. The thickness of ViFLEX-L was 50 μm, the melting point was 280 °C, Td1 was 240 °C, and Td2 was 260 °C ( Figure 3 , the rheological curve of ViFLEX-L is obtained by the above-mentioned high temperature inflection point and low temperature inflection point test methods); the thickness of ViFLEX-M is 50μm, the melting point is 310℃, Td1 is 265℃, and Td2 is 288℃.
[0060] 2. Aluminum foil:
[0061] Aluminum foil 1: brand 8007, bonding surface roughness Rz is 2.8μm; aluminum foil 2: brand 8021, bonding surface roughness Rz is 1.8μm; aluminum foil 3: brand 1060, roughness Rz is 1.2μm; the above aluminum foils are all purchased from Henan Mingtai Aluminum Co., Ltd.; coated with a silicone release layer, the release agent brand is Lub O 32F, and dried at 150°C before use.
[0062] Example 1
[0063] A roller press was used to heat-press the LCP film (brand name ViFLEX-L) and two layers of 8021 aluminum foil (already coated with a release agent) to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. The aluminum foil on one side (i.e., one layer) of the obtained laminate was peeled off using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.) (Note: "loosening the film" in the present invention means using a film elastic winding machine to make the layers of the film coil non-contact, the same below), and the obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment (during the heat treatment, the film coils were placed vertically, and nitrogen was circulated and purged in the vertical direction, see Figure 1 ; the same below), then the first sampling was carried out and its melting point, low-temperature inflection point and high-temperature inflection point were determined (Note: sampling is to take out only a small amount of samples for determination, and the remaining samples do not need to be taken out, and the temperature is continued to be raised to increase the melting point, the same below), the melting point was increased to 303°C, Td1′ was 265°C, and Td2′ was 284°C; then the oven temperature was increased to 280°C, and the remaining samples after the first sampling were continued to be heat treated for 2h for the second stage of melting point increase, the second sampling was carried out and the melting point, low-temperature inflection point and high-temperature inflection point were determined, the melting point was increased to 319°C, Td1″ was 275°C, and Td2″ was 294°C; the oven temperature was increased to 285°C again, and the remaining samples after the second sampling were continued to be heat treated for 4h for the third stage of melting point increase, the third sampling was carried out and the melting point was determined, and the melting point was increased to 334°C; finally, the oven was cooled to 150°C at a rate of 10°C / min, and the film samples were taken out. The film sample was tightened with a film tensioner (Note: the "tightening the film" in the present invention means using a film tensioner to restore the film coil to the state before the film was loosened, the same below), and then the other layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0064] Example 2
[0065] The ViFLEX-L film and two layers of 8021 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 250°C, the pressure was 1 ton, and the speed was 1 m / min. One layer of the aluminum foil was peeled off from the obtained laminate using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment, and then the first sampling was performed to determine its melting point, low-temperature inflection point, and high-temperature inflection point. Its melting point was increased to 303°C, T d1′ is 265°C, Td2′ is 284°C; then the oven temperature is increased to 280°C, and the remaining samples after the first sampling are heat treated for 2h for the second stage of melting point increase. The second sampling is carried out and the melting point, low-temperature inflection point and high-temperature inflection point are measured, and the melting point is increased to 319°C. Td1″ is 275°C, and Td2″ is 294°C; then the oven temperature is increased to 285°C, and the remaining samples after the second sampling are heat treated for 4h for the third stage of melting point increase. The third sampling is carried out and the melting point is measured, and the melting point is increased to 334°C; finally, the oven is cooled to 150°C at a rate of 10°C / min, and the film samples are taken out. The film sample was rolled up tightly with a film elastic winding machine, and then the other layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0066] Example 3
[0067] The ViFLEX-L film and two layers of 8021 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1.5 tons, and the speed was 1 m / min. One layer of the aluminum foil in the obtained laminate was peeled off using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment, and then the first sampling was performed to measure its melting point, low-temperature inflection point, and high-temperature inflection point. Its melting point was increased to 303°C. Td1′ is 265°C, Td2′ is 284°C; then the oven temperature is increased to 280°C, and the remaining samples after the first sampling are heat treated for 2 hours for the second stage of melting point increase. The second sampling is carried out and the melting point, low-temperature inflection point and high-temperature inflection point are measured, and the melting point is increased to 319°C. Td1″ is 275°C, and Td2″ is 294°C; then the oven temperature is increased to 285°C, and the remaining samples after the second sampling are heat treated for 4 hours for the third stage of melting point increase. The third sampling is carried out and the melting point is measured, and the melting point is increased to 334°C; finally, the oven is cooled to 150°C at a rate of 10°C / min, and the film samples are taken out. The film sample was rolled up tightly with a film elastic winding machine, and then the other layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0068] Example 4
[0069] The ViFLEX-L film and two layers of 8021 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. One layer of the aluminum foil was peeled off from the obtained laminate using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 250°C for 6 hours) for the first stage of heat treatment, and then the first sampling was performed to determine its melting point, low-temperature inflection point, and high-temperature inflection point. Its melting point was increased to 296°C, T d1′ is 261°C, Td2′ is 279°C; then the oven temperature is increased to 275°C, and the remaining samples after the first sampling are heat treated for 4 hours for the second stage of melting point increase. The second sampling is carried out and the melting point, low-temperature inflection point and high-temperature inflection point are measured, and the melting point is increased to 308°C, Td1″ is 272°C, and Td2″ is 296°C; then the oven temperature is increased to 285°C, and the remaining samples after the second sampling are heat treated for 6 hours for the third stage of melting point increase. The third sampling is carried out and the melting point is measured, and the melting point is increased to 332°C; finally, the oven is cooled to 150°C at a rate of 10°C / min, and the film samples are taken out. The film sample was rolled up tightly with a film elastic winding machine, and then the other layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0070] Example 5
[0071] The LCP film (brand name ViFLEX-M) and two layers of 8021 aluminum foil (coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 300°C, the pressure was 1 ton, and the speed was 1 m / min. Subsequently, the aluminum foil on one side (i.e., one layer) of the obtained laminate was peeled off using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.), and the obtained sample was placed in a high-temperature oxygen-free oven for baking (28 0℃ for 4h) for the first stage of heat treatment, then the first sampling was carried out and its melting point, low temperature inflection point and high temperature inflection point were measured, and its melting point was raised to 324℃, Td1′ was 292℃, and Td2′ was 311℃; then the oven temperature was raised to 300℃, and the remaining samples after the first sampling were further heat treated for 4h for the second stage of melting point increase, and the second sampling was carried out and its melting point was measured, and its melting point was raised to 336℃; finally, the oven was cooled to 150℃ at a rate of 10℃ / min, and the film sample was taken out. The film sample was inverted with a film elastic winding machine, and then another layer of aluminum foil was peeled off with a slitting machine, and then 18μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for double-sided hot pressing copper cladding, the hot pressing temperature was 340℃, the pressure was 3MPa, and the time was 6min to obtain a flexible copper clad laminate (FCCL), and its performance test results are shown in Table 1.
[0072] Comparative Example 1
[0073] The ViFLEX-L film and two layers of 1060 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. One layer of the aluminum foil was peeled off from the obtained laminate using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment, and then the first sampling was performed to determine its melting point, low-temperature inflection point, and high-temperature inflection point. Its melting point was increased To 303℃, Td1′ is 265℃, Td2′ is 284℃; then the oven temperature is increased to 280℃, and the remaining samples after the first sampling are heat treated for 2h for the second stage of melting point increase, and the second sampling is carried out and its melting point as well as the low-temperature inflection point and the high-temperature inflection point are measured, and its melting point is increased to 319℃, Td1″ is 275℃, and Td2″ is 294℃; then the oven temperature is increased to 285℃, and the remaining samples after the second sampling are heat treated for 4h for the third stage of melting point increase, and the melting point is increased to 334℃; finally, the oven is cooled to 150℃ at a rate of 10℃ / min, and the film samples are taken out. The film sample was rolled up tightly with a film elastic winding machine, and then the other layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0074] Comparative Example 2
[0075] The ViFLEX-L film and two layers of 8007 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. One layer of the aluminum foil was peeled off from the obtained laminate using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment, and then the first sampling was performed to determine its melting point, low-temperature inflection point, and high-temperature inflection point. The melting point was increased To 303℃, Td1′ is 265℃, Td2′ is 284℃; then the oven temperature is increased to 280℃, and the remaining samples after the first sampling are heat treated for 2h for the second stage of melting point increase, and the second sampling is carried out and its melting point as well as the low-temperature inflection point and the high-temperature inflection point are measured, and its melting point is increased to 319℃, Td1″ is 275℃, and Td2″ is 294℃; then the oven temperature is increased to 285℃, and the remaining samples after the second sampling are heat treated for 4h for the third stage of melting point increase, and the melting point is increased to 334℃; finally, the oven is cooled to 150℃ at a rate of 10℃ / min, and the film samples are taken out. The film sample was rolled up tightly with a film elastic winding machine, and then the other layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0076] Comparative Example 3
[0077] The ViFLEX-L film and two layers of 8021 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. One layer of the aluminum foil in the obtained laminate was peeled off using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment, and then the first sampling was performed to determine its melting point and The low-temperature inflection point and the high-temperature inflection point, the melting point is increased to 303°C, Td1′ is 265°C, and Td2′ is 284°C; then the oven temperature is increased to 280°C, and the remaining samples after the first sampling are heat treated for 2 hours for the second stage of melting point increase, and the second sampling is carried out and the melting point as well as the low-temperature inflection point and the high-temperature inflection point are measured, and the melting point is increased to 319°C, Td1″ is 275°C, and Td2″ is 294°C; then the oven temperature is increased to 285°C, and the remaining samples after the second sampling are heat treated for 4 hours for the third stage of melting point increase, and the melting point is increased to 334°C. The film sample was taken out directly, cooled in the air, and then tightened with a film elastic winder. After that, the other layer of aluminum foil was peeled off with a slitter, and then 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding. The hot pressing temperature was 340 ° C, the pressure was 3 MPa, and the time was 6 min to obtain a flexible copper clad laminate (FCCL). The performance test results are shown in Table 1.
[0078] Comparative Example 4
[0079] ViFLEX-L film and two layers of 8021 aluminum foil (already coated with release agent) were hot pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the laminating temperature was 260°C, the pressure was 1 ton, and the speed was 1m / min. The laminate was peeled off one layer of aluminum foil using a slitter. The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4h), and then the oven temperature was raised to 280°C for heat treatment for 2h; then the oven temperature was raised to 285°C for heat treatment for 4h; finally, the oven was cooled to 150°C at a rate of 10°C / min, and the film sample was taken out. After the other layer of aluminum foil was peeled off using a slitter, 18μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding to obtain a flexible copper clad laminate (FCCL), the hot pressing temperature was 340°C, the pressure was 3MPa, and the time was 6min. The performance test results are shown in Table 1.
[0080] Comparative Example 5
[0081] The ViFLEX-L film was hot-pressed with a single layer of 8021 aluminum foil (already coated with release agent) using a roller press, the laminating temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. The obtained laminate was placed in a high-temperature oxygen-free oven for baking (baking at 260°C for 4 hours) for the first stage of heat treatment, and then the first sampling was carried out to measure its melting point, low-temperature inflection point and high-temperature inflection point. The melting point was raised to 303°C, Td1′ was 265°C, and Td2′ was 284°C. The oven temperature was then raised to 2 80℃, continue heat treatment for 2h for the remaining samples after the first sampling to increase the melting point in the second stage, take samples for the second time and measure their melting point, low temperature inflection point and high temperature inflection point, the melting point is increased to 319℃, Td1″ is 275℃, Td2″ is 294℃; then increase the oven temperature to 285℃, continue heat treatment for 4h for the remaining samples after the second sampling to increase the melting point in the third stage, the melting point is increased to 334℃; finally, cool the oven to 150℃ at a rate of 10℃ / min, and take out the film sample. After peeling off the aluminum foil with a slitting machine, use 18μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) for hot pressing double-sided copper cladding, the hot pressing temperature is 340℃, the pressure is 3MPa, and the time is 6min to obtain a flexible copper clad laminate (FCCL), and its performance test results are shown in Table 1.
[0082] Comparative Example 6
[0083] The ViFLEX-L film and two layers of 8021 aluminum foil (already coated with release agent) were hot-pressed and laminated using a roller press to form an Al-LCP film-Al laminate, wherein the lamination temperature was 260°C, the pressure was 1 ton, and the speed was 1 m / min. One layer of the aluminum foil was peeled off using a slitting machine, and then the film was loosened using a film elastic winding machine (TL-101, Jingzhong Enterprise Co., Ltd.). The obtained sample was placed in a high-temperature oxygen-free oven for baking (baking at 270°C for 2 hours) for the first stage of heat treatment, and then the first sampling was performed to determine its melting point, low-temperature inflection point, and high-temperature inflection point. Its melting point was increased To 307℃, Td1′ is 271℃, Td2′ is 289℃; then the oven temperature is increased to 295℃, and the remaining samples after the first sampling are heat treated for 2h for the second stage of melting point increase, and the second sampling is carried out and the melting point as well as the low-temperature inflection point and the high-temperature inflection point are measured, and the melting point is increased to 328℃, Td1″ is 290℃, and Td2″ is 305℃; then the oven temperature is increased to 300℃, and the remaining samples after the second sampling are heat treated for 1h for the third stage of melting point increase, and the melting point is increased to 337℃; finally, the oven is cooled to 150℃ at a rate of 10℃ / min, and the film samples are taken out. The sample was rolled up tight with a film elastic winding machine, and then another layer of aluminum foil was peeled off with a slitting machine. Then, 18 μm electrolytic copper foil (Futian copper foil, brand RCF-TNBG-HP) was used for hot pressing of double-sided copper cladding to obtain a flexible copper clad laminate (FCCL). The hot pressing temperature was 342 ° C, the pressure was 3 MPa, and the time was 6 min. The performance test results are shown in Table 1.
[0084] Table 1
[0085]
[0086] From the results in Table 1, it can be seen that after two-stage or three-stage melting point raising using the method of the present invention, the melting point can be raised to 332-336°C (Examples 1-5), while the performance under other conditions (Comparative Examples 1-6) is far inferior to that of the present invention.
[0087] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for producing a high melting point LCP film, characterized in that: The steps include: (1) Pressing aluminum: hot pressing the LCP film and two layers of aluminum foil with a roughness of 1.5 μm to 2 μm to form an aluminum foil-LCP film-aluminum foil laminate; wherein the hot pressing temperature is 10 to 30°C below the melting point of the LCP film, the pressure is 0.5 to 1.5 tons, and the speed is 0.5 to 1.5 m / min; (2) Step-by-step temperature increase to improve melting point: ① After peeling off one layer of the aluminum foil of the aluminum foil-LCP film-aluminum foil laminate obtained in step (1) using a slitting machine, loosen the LCP film coil using a film tensioning and winding machine, and then place the obtained sample in a high-temperature oxygen-free oven, bake it in the temperature range of the low-temperature inflection point Td1 to the high-temperature inflection point Td2 of the LCP film for 4 to 6 hours to perform the first stage of melting point increase, and then perform the first sampling and measure the melting point, low-temperature inflection point Td1′ and high-temperature inflection point Td2′ of the sample; if the melting point is increased to above 330°C, stop here and obtain the high-melting-point LCP film; if the melting point is lower than 330°C, proceed to the next step; ② The remaining samples after the first sampling are further heated to Td1′~Td2′ and heat treated for 2~6 hours to increase the melting point in the second stage, and then the second sampling is performed to measure the melting point, low temperature inflection point Td1″ and high temperature inflection point Td2″ of the samples; if the melting point is increased to above 330°C, the process ends here and the high melting point LCP film is obtained; if the melting point is lower than 330°C, the process proceeds to the next step; ③ Repeat step ② until the melting point is raised to above 330°C; after the heat treatment is completed, cool to 150°C, take out the film, and use a film tension winder to tighten the film, and then use a slitting machine to peel off the other layer of aluminum foil to obtain the high melting point LCP film.
2. The method for producing a high melting point LCP film according to claim 1, wherein: The aluminum foil in step (1) has been coated with a release agent; The release agent is a silicone release agent; In step (2), during the heat treatment, the LCP film coil is placed vertically and nitrogen is circulated and purged in the vertical direction.
3. The method for producing a high melting point LCP film according to claim 1, wherein: In step (1), the temperature of hot pressing bonding is 20 to 30° C. below the melting point of the LCP film; In step (1), the pressure of hot pressing is 0.5 to 1.5 tons; The cooling rate in step (2) is below 10°C / min.
4. The method for producing a high melting point LCP film according to claim 1, wherein: In step (2), the heat treatment temperature of each stage is between the low-temperature inflection point and the high-temperature inflection point of the LCP film, wherein the low-temperature inflection point and the high-temperature inflection point are measured by rotational rheology. When the sample is heated at 5°C / min to the melting point of the sample, its storage modulus versus temperature curve has two inflection points, which are recorded as the low-temperature inflection point and the high-temperature inflection point from low to high temperatures, respectively.
5. The method for producing a high melting point LCP film according to claim 1, wherein: The LCP film described in step (1) has a thickness of 25 to 100 μm, a melting point of 280 to 310° C., Td1 of 240 to 265° C., and Td2 of 260 to 288° C.
6. A high melting point LCP film, characterized in that: It is produced by the method according to any one of claims 1 to 5.
7. Application of the high melting point LCP film according to claim 6 in high frequency and high speed communication substrates, millimeter wave radars, airborne, missile-borne or satellite-borne equipment.
8. The use according to claim 7, characterized in that: The high-frequency and high-speed communication substrate includes a flexible copper-clad laminate and / or a flexible printed circuit board; The millimeter wave radar includes a military millimeter wave radar.
9. A flexible copper-clad laminate, characterized in that: It comprises the high melting point LCP film as claimed in claim 6 and electrolytic copper foil.
10. The method for preparing the flexible copper clad laminate according to claim 9, characterized in that: The method comprises the following steps: hot pressing the high melting point LCP film according to claim 6 and the electrolytic copper foil to coat copper on both sides, the hot pressing temperature is 340-345° C., the pressure is 2-4 MPa, and the hot pressing time is 5-10 min, to obtain the product; The thickness of the electrolytic copper foil is 12-18 μm.