Laser-processed micro-nano composite structure with anti-icing and de-icing effects and preparation method of micro-nano composite structure

Micro-nano composite structures are prepared through femtosecond laser processing, combined with polydimethylsiloxane materials doped with lubricating liquid, which solves the energy consumption and inefficiency problems of traditional anti-icing methods, and achieves high durability and low cost removal. Ice effect, ice adhesion strength is significantly reduced, the icing time is prolonged, and good ice-removing performance is maintained after multiple cycles.

CN118908142APending Publication Date: 2024-11-08SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014994.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional anti-icing methods have problems of energy consumption, environmental pollution and inefficiency, and commonly used lubricants are easily lost during deicing and rainwater erosion, resulting in anti-icing/deicing failure.

Method used

Femtosecond laser processing is used to prepare a liquid injection surface with reversible temperature response on a polytetrafluoroethylene sheet. By forming a micro-column array and a micro-cone array structure on its surface, combined with a polydimethylsiloxane material doped with lubricating liquid. Form a high-durability micro-nano composite structure to reduce ice adhesion strength and improve ice-sparing effect.

Benefits of technology

Achieve high durability and low cost anti-icing effect, the ice adhesion strength is reduced to 2.51kPa, the icing time is extended to 1033s, and the good ice-bleaning performance is maintained after multiple icing and deicing cycles, which is important. Application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908142A_ABST
    Figure CN118908142A_ABST
Patent Text Reader

Abstract

The invention discloses a micro-nano composite structure with anti-icing and deicing effects for laser processing and a preparation method thereof, and relates to the field of material surface laser processing, the micro-nano composite structure comprises a liquid injection surface with reversible temperature response, a micro-column array is arranged on the surface of the liquid injection surface, the micro-column array comprises a plurality of micro-column structures arranged in a periodic array, and the micro-column structures are arranged on the surface of the liquid injection surface; the top end of each micro-column structure is provided with a micro-cone array through laser processing, and each micro-cone array comprises a plurality of micro-cone structures which are arranged in a periodic array. The micro-nano composite structure provided by the invention has a good ice dredging effect, and can simultaneously realize good ice prevention, ice dredging and durability. In the anti-icing aspect, the micro-nano composite structure has a smaller solid-liquid contact area, so that the heat transfer efficiency can be effectively reduced, the freezing of water drops on the surface of the micro-nano composite structure is delayed, and the longest freezing time can reach 1033s; in the aspect of ice dredging, the ice adhesion strength of the surface can be as low as 2.51 kPa; in the aspect of durability, after the surface is iced and deiced for multiple times, the micro-nano composite structure basically remains unchanged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of laser processing and anti-icing of material surfaces, and more specifically, to a laser-processed micro-nano composite structure with anti-icing effect and a preparation method thereof. Background Art

[0002] Ice accumulation is prone to occur in cold regions, which can cause serious safety accidents and significant economic losses in many fields, including power transmission, communications, energy, and transportation. Therefore, it is urgent to develop efficient anti-icing / de-icing strategies to solve the ice accumulation problem. Generally speaking, traditional active de-icing technologies such as mechanical methods, electrothermal methods, photothermal methods, and chemical methods will inevitably bring about problems such as energy consumption, environmental pollution, and low efficiency. Compared with traditional methods, it is urgent to find more efficient, environmentally friendly, and economical anti-icing and de-icing methods.

[0003] Inspired by the natural pitcher plant, slippery liquid-infused porous surface (SLIPS) has attracted much attention due to its excellent water repellency and anti-icing properties. SLIPS has a stable lubricating layer between the droplet and the sample surface; this lubricating layer isolates the solid surface from the droplet, inhibits the formation of ice crystal nucleation, and greatly reduces the adhesion strength of ice. However, during deicing and rain erosion, the surface lubricant is easily lost, resulting in anti-icing / de-icing failure. In order to reduce the migration of lubricants and improve durability, soft elastomers are widely used as one of the effective materials to solve ice accumulation. Therefore, it is also crucial to develop a slippery liquid-infused surface that has both effective anti-icing durability and flexibility through a simple method. Summary of the invention

[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0005] In order to achieve these purposes and other advantages according to the present invention, a laser-processed micro-nano composite structure with anti-icing effect is provided, comprising:

[0006] A liquid injection surface with reversible temperature response is provided on the surface, wherein a microcolumn array is provided, wherein the microcolumn array includes a plurality of microcolumn structures arranged in a periodic array, wherein the top of each microcolumn structure is provided with a microcone array by laser processing, wherein the microcone array includes a plurality of microcone structures arranged in a periodic array.

[0007] Preferably, the liquid injection surface having a reversible temperature response is a transparent flexible surface.

[0008] Preferably, the diameter of the micro-cone structure is 28 to 32 μm, and the center spacing between the micro-cone structures is 28 to 32 μm; each of the micro-column structures is distributed in a square, the height of the micro-column structure is 380 to 400 μm, the diameter is 145 to 155 μm, and the spacing between two adjacent micro-column structures is 149 to 151 μm.

[0009] A method for preparing a laser-processed micro-nano composite structure with an anti-icing effect comprises the following steps:

[0010] S1. Using a femtosecond laser to process a plurality of through holes on a polytetrafluoroethylene sheet having a thickness of 400 μm, wherein each of the through holes is distributed in a square shape;

[0011] S2, cleaning the processed polytetrafluoroethylene sheet in anhydrous ethanol for ten minutes and drying it to obtain a micro-column template;

[0012] S3, spraying a release agent on the micro-column template obtained in S2, then pouring a liquid injection material with a reversible temperature response into the micro-column template to cover the micro-column template by 700-800 μm, and placing the micro-column template filled with the liquid injection material with a reversible temperature response into a drying oven at a temperature of 80-120° C. for curing for 1-4 hours and then demolding to obtain a micro-column array on the liquid injection surface with a reversible temperature response;

[0013] S4. Use a femtosecond laser to scan the liquid injection surface with the microcolumn array obtained in S3. The incident direction of the laser beam is perpendicular to the liquid injection surface. Grid line scanning is performed on the surface of a single microcolumn structure. A microcone array is processed at the top of the microcolumn structure to obtain a micro-nano composite structure.

[0014] Preferably, the material of the liquid-injected surface having a reversible temperature response is polydimethylsiloxane doped with 60 wt % of a mixed lubricating liquid.

[0015] Preferably, the lubricating liquid is prepared by mixing silicone oil and liquid paraffin in a mass ratio of 1:1, wherein the viscosity of the silicone oil is 100 mm 2 / s.

[0016] Preferably, in S1, the diameter of the through holes is 145-155 μm, and the spacing is 149-151 μm.

[0017] Preferably, in S4, the pulse energy of the femtosecond laser is 20-30 mW, and the scanning speed is 0.001 m·s -1 , the scanning grid line spacing is 28 to 32 μm.

[0018] The invention discloses an application of a laser processed micro-nano composite structure with an anti-icing effect. The micro-nano composite structure with a high-durability anti-icing effect is applied to the field of anti-icing and deicing.

[0019] Preferably, the liquid injection surface with reversible temperature response is adhered to the surface of the required anti-icing and de-icing structure, and is used for anti-icing and de-icing on the surface of the required anti-icing and de-icing structure.

[0020] The present invention has at least the following beneficial effects:

[0021] 1. The preparation method of the micro-nano composite structure with high durability anti-icing effect provided by the present invention imitates the super hydrophobicity of lotus leaves and the lubricating surface of pitcher plants, adopts femtosecond laser processing, prepares a through-hole structure with precise and controllable morphology on a polytetrafluoroethylene sheet, obtains a micro-pillar array structure through transfer printing, and finally, through femtosecond laser processing, the top of the micro-pillar structure presents a micro-cone array structure. The micro-nano composite structure reduces the contact area between the micro-droplets and the droplets, and at the same time, lubricating fluid will be secreted at low temperatures, reducing the ice adhesion strength, thereby achieving a good ice-repelling effect.

[0022] 2. The present invention utilizes cutting-edge bionic principles, has a simple preparation process, low cost, and can precisely control the structure, so that it can achieve efficient and large-area preparation, and can simultaneously achieve good anti-icing, ice-repelling, and durability. In terms of anti-icing, the micro-nano composite structure has a smaller solid-liquid contact area, which can effectively reduce the heat transfer efficiency and delay the freezing of water droplets on its surface, with the longest freezing time up to 1033s; in terms of ice repelling, the ice adhesion strength on the surface can be as low as 2.51 kPa. The low ice adhesion strength can quickly remove the ice on the surface under the action of external forces such as tilt, breeze, and vibration, thereby maintaining a good ice repelling effect; in terms of durability, after multiple ice and de-icing cycles, the micro-nano composite structure of the surface remains basically unchanged, and even after multiple ice and de-icing cycles, its ice adhesion strength can still be maintained below 20 kPa, and it can be reused many times, which has important application potential in the field of anti-icing and de-icing.

[0023] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of a micro-nano composite structure with anti-icing effect processed by laser according to the present invention;

[0025] Figure 2 Electron microscope images of micro-pillars and micro-cones of the micro-nano composite structure with anti-icing effect processed by laser according to the present invention;

[0026] Figure 3This is a static anti-icing function diagram of the micro-nano composite structure with anti-icing effect processed by laser in Example 1;

[0027] Figure 4 This is an electron microscope image of the laser-processed micro-nano composite structure with anti-icing effect after 50 icing and deicing cycles in Example 3;

[0028] Figure 5 It is a bar graph of low ice adhesion strength of Comparative Examples 1-2 and Example 3 of the present invention;

[0029] Figure 6 It is a durability diagram of ice formation and deicing cycles of comparative example 1 and embodiment 3 of the present invention.

[0030] The corresponding structure names are marked in the figure: 1-micro-column structure; 2-micro-cone structure. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0032] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0033] The microstructure of the lotus leaf surface makes it hydrophobic, providing an air layer between the solid surface and the liquid droplets, which correspondingly reduces the actual contact area and prevents heat conduction. The smooth liquid injected into the surface inspired by the pitcher plant, because of the presence of the lubricating layer, ice can easily slide off the surface under the action of external force or vibration, and it can also inhibit the formation of ice nuclei.

[0034] The present invention imitates the surface of lotus leaf and pitcher plant, and uses femtosecond laser processing combined with transfer printing to process a micro-nano composite structure on the surface of liquid injection with reversible temperature response, including using femtosecond laser to process periodically distributed through holes and micro-cone structures, and using transfer printing to form a periodically distributed micro-column structure on the surface (see Figure 2 ), a micro-nano composite structure with high durability and anti-icing effect is obtained.

[0035] The diameter of the microcones is 28-32 μm, and the center spacing between the microcones is 28-32 μm; each microcolumn is distributed in a square shape, the height of the microcolumn is 380-400 μm, the diameter is 145-155 μm, and the spacing between two adjacent microcolumns is 149-151 μm. It has reversible thermal responsiveness. At low temperatures, its surface will become turbid and secrete lubricating fluid; at high temperatures, the surface will become transparent, the lubricating fluid will be absorbed back, and the hydrophobicity will be further improved.

[0036] The specific scheme proposed by the present invention is described in more detail with reference to several specific embodiments below.

[0037] Example 1

[0038] like Figure 1 As shown, this embodiment provides a laser-processed micro-nano composite structure with high durability and anti-icing effect, including:

[0039] A liquid injection surface with a reversible temperature response is provided on the surface, wherein a microcolumn array is provided, wherein the microcolumn array comprises a plurality of microcolumn structures 1 arranged in a periodic array, wherein the top of each of the microcolumn structures 1 is provided with a microcone array by laser processing, wherein the microcone array comprises a plurality of microcone structures 2 arranged in a periodic array.

[0040] The material of the liquid injection surface with reversible temperature response is polydimethylsiloxane doped with 60wt% mixed lubricant; the lubricant is a mixture of silicone oil and liquid paraffin in a mass ratio of 1:1, and the viscosity of the silicone oil is 100mm 2 / s.

[0041] The diameter of the micro-cone structure 2 is 28-32 μm, and the center distance between the micro-cone structures 2 is 28-32 μm; each of the micro-column structures 1 is distributed in a square, the height of the micro-column structure 1 is 380-400 μm, the diameter is 145-155 μm, and the distance between two adjacent micro-column structures 1 is 149-151 μm.

[0042] The method for preparing the micro-nano composite structure with high durability anti-icing effect of this embodiment comprises the following steps:

[0043] S1. Using a femtosecond laser to process a plurality of through holes on a polytetrafluoroethylene sheet having a thickness of 400 μm, wherein each of the through holes is distributed in a square shape;

[0044] S2, cleaning the processed polytetrafluoroethylene sheet in anhydrous ethanol for ten minutes and drying it to obtain a micro-column template;

[0045] S3, spraying a release agent on the micro-column template obtained in S2, then pouring a liquid injection material with a reversible temperature response into the micro-column template to cover the micro-column template by 700-800 μm, and placing the micro-column template filled with the liquid injection material with a reversible temperature response into a drying oven at a temperature of 120° C. for curing for 2 hours and then demoulding to obtain a micro-column array on the liquid injection surface with a reversible temperature response;

[0046] S4, using a femtosecond laser to scan the liquid injection surface with a micro-column array obtained in S3, with the incident direction of the laser beam perpendicular to the liquid injection surface, performing grid line scanning on the surface of a single micro-column structure, and processing a micro-cone array at the top of the micro-column structure to obtain a micro-nano composite structure. The pulse energy of the femtosecond laser is 25mW, and the scanning speed is 0.001m·s -1 , the scanning grid line spacing is 28~32μm

[0047] See also Figure 3 ,In order to verify the anti-icing effect of the micro-nano composite structure with high ,durability anti-icing effect, the sample was horizontally pasted on the refrigeration table, a drop of 10μL ultrapure water was dropped on the surface of the micro-nano composite structure with high ,durability anti-icing effect, the power of the refrigeration table was turned on, and the time for the drop to be completely frozen was 1033s.

[0048] Example 2

[0049] This embodiment provides a laser-processed micro-nano composite structure with high durability and anti-icing effect, including:

[0050] A liquid injection surface with a reversible temperature response is provided on the surface, wherein a microcolumn array is provided, wherein the microcolumn array comprises a plurality of microcolumn structures 1 arranged in a periodic array, wherein the top of each of the microcolumn structures 1 is provided with a microcone array by laser processing, wherein the microcone array comprises a plurality of microcone structures 2 arranged in a periodic array.

[0051] The material of the liquid injection surface with reversible temperature response is polydimethylsiloxane doped with 60wt% mixed lubricant; the lubricant is a mixture of silicone oil and liquid paraffin in a mass ratio of 1:1, and the viscosity of the silicone oil is 100mm 2 / s.

[0052] The diameter of the micro-cone structure 2 is 28-32 μm, and the center distance between the micro-cone structures 2 is 28-32 μm; each of the micro-column structures 1 is distributed in a square, the height of the micro-column structure 1 is 380-400 μm, the diameter is 145-155 μm, and the distance between two adjacent micro-column structures 1 is 149-151 μm.

[0053] The method for preparing the micro-nano composite structure with high durability anti-icing effect of this embodiment comprises the following steps:

[0054] S1. Using a femtosecond laser to process a plurality of through holes on a polytetrafluoroethylene sheet having a thickness of 400 μm, wherein each of the through holes is distributed in a square shape;

[0055] S2, cleaning the processed polytetrafluoroethylene sheet in anhydrous ethanol for ten minutes and drying it to obtain a micro-column template;

[0056] S3, spraying a release agent on the micro-column template obtained in S2, then pouring a liquid injection material with a reversible temperature response into the micro-column template to cover the micro-column template by 700-800 μm, and placing the micro-column template filled with the liquid injection material with a reversible temperature response into a drying oven at a temperature of 120° C. for curing for 2 hours and then demoulding to obtain a micro-column array on the liquid injection surface with a reversible temperature response;

[0057] S4, using a femtosecond laser to scan the liquid injection surface with a micro-column array obtained in S3, with the incident direction of the laser beam perpendicular to the liquid injection surface, performing grid line scanning on the surface of a single micro-column structure, and processing a micro-cone array at the top of the micro-column structure to obtain a micro-nano composite structure. The pulse energy of the femtosecond laser is 25mW, and the scanning speed is 0.001m·s -1 , the scanning grid line spacing is 28 to 32 μm.

[0058] In order to verify the ice-repellent performance of the micro-nano composite structure with high durability anti-icing effect, the sample was placed horizontally in a refrigerator at a temperature of -25°C and a relative humidity of 80%. A transparent uncovered square tube of 8mm×8mm×30mm was used as a mold and placed on the sample. Ultrapure water was added to the mold and frozen for 1h until it was completely frozen, and then the icicle was pushed at a constant speed with a thrust gauge. The peak force required to push down the icicle was recorded, and its ice adhesion strength was calculated to be 2.51kPa.

[0059] Example 3

[0060] This embodiment provides a laser-processed micro-nano composite structure with high durability and anti-icing effect, including:

[0061] A liquid injection surface with a reversible temperature response is provided on the surface, wherein a microcolumn array is provided, wherein the microcolumn array comprises a plurality of microcolumn structures 1 arranged in a periodic array, wherein the top of each of the microcolumn structures 1 is provided with a microcone array by laser processing, wherein the microcone array comprises a plurality of microcone structures 2 arranged in a periodic array.

[0062] The material of the liquid injection surface with reversible temperature response is polydimethylsiloxane doped with 60wt% mixed lubricant; the lubricant is a mixture of silicone oil and liquid paraffin in a mass ratio of 1:1, and the viscosity of the silicone oil is 100mm 2 / s.

[0063] The diameter of the micro-cone structure 2 is 28-32 μm, and the center distance between the micro-cone structures 2 is 28-32 μm; each of the micro-column structures 1 is distributed in a square, the height of the micro-column structure 1 is 380-400 μm, the diameter is 145-155 μm, and the distance between two adjacent micro-column structures 1 is 149-151 μm.

[0064] The method for preparing the micro-nano composite structure with high durability anti-icing effect of this embodiment comprises the following steps:

[0065] S1. Using a femtosecond laser to process a plurality of through holes on a polytetrafluoroethylene sheet having a thickness of 400 μm, wherein each of the through holes is distributed in a square shape;

[0066] S2, cleaning the processed polytetrafluoroethylene sheet in anhydrous ethanol for ten minutes and drying it to obtain a micro-column template;

[0067] S3, spraying a release agent on the micro-column template obtained in S2, then pouring a liquid injection material with a reversible temperature response into the micro-column template to cover the micro-column template by 700-800 μm, and placing the micro-column template filled with the liquid injection material with a reversible temperature response into a drying oven at a temperature of 120° C. for curing for 2 hours and then demoulding to obtain a micro-column array on the liquid injection surface with a reversible temperature response;

[0068] S4, using a femtosecond laser to scan the liquid injection surface with a micro-column array obtained in S3, with the incident direction of the laser beam perpendicular to the liquid injection surface, performing grid line scanning on the surface of a single micro-column structure, and processing a micro-cone array at the top of the micro-column structure to obtain a micro-nano composite structure. The pulse energy of the femtosecond laser is 25mW, and the scanning speed is 0.001m·s -1 , the scanning grid line spacing is 28 to 32 μm.

[0069] In order to verify the durable cyclic performance of the micro-nano composite structure with high durability anti-icing effect, the sample was placed horizontally in a refrigerator at a temperature of -25°C and a relative humidity of 80%. A transparent uncovered square tube of 8mm×8mm×30mm was used as a mold and placed on the sample. Ultrapure water was added to the mold and frozen for 1 hour until it was completely frozen. Then the icicle was pushed at a constant speed with a thrust gauge, and the peak force required to push down the icicle was recorded. The period from the complete freezing of the icicle to the pushing down of the icicle was regarded as an icing and deicing cycle. After 50 cycles, although some structures on the surface were damaged, the overall composite micro-nano structure was not significantly damaged (see Figure 4 ).

[0070] Through the verification of the above-mentioned embodiments 1 to 3, embodiment 1 can achieve the best anti-icing effect, and the ice extension time can be close to 1033s; embodiment 2 can achieve the best ice-repelling effect, and the lowest ice adhesion strength is 2.51kPa; embodiment 3 can achieve the best durability effect. After multiple ice formation and deicing cycles, the overall micro-nano composite structure has no obvious damage. Good anti-icing, ice-repelling and durability have important application value in the field of anti-icing and deicing.

[0071] In order to better illustrate the beneficial effects that can be achieved by the micro-nano composite structure with high durability anti-icing effect and the preparation method thereof of the present invention, the technical solution of the present invention is further analyzed with several comparative examples below.

[0072] Comparative Example 1

[0073] This comparative example is a liquid injection surface with reversible temperature response without processing any structure, and the material of the liquid injection surface with reversible temperature response is the same as that of Examples 1 to 3, and other conditions remain unchanged.

[0074] In order to test the anti-icing effect of the surface of the structure in this comparative example, the sample was horizontally pasted on a cooling table, a drop of 10 μL of ultrapure water was dropped on the surface of the structure, and the power of the cooling table was turned on. The freezing time of the droplets on the surface of the structure without structure in this comparative example was calculated to be 649 s.

[0075] Comparative Example 2

[0076] This comparative example provides a micro-nano composite structure, and the structure of its microcolumn array and microcone array is the same as that of Example 1 to Example 3, except that the lubricating liquid in Example 1 to Example 3 is not added to the material of the liquid injection surface with reversible temperature response in this comparative example, and the other structural parameters are the same as those of Example 1 to Example 3.

[0077] See also Figure 5 In order to verify the ice-repellent performance of Comparative Examples 1 to 2, the samples were placed horizontally in a refrigerator at a temperature of -25°C and a relative humidity of 80%. A transparent uncovered square tube of 8mm×8mm×30mm was used as a mold and placed on the sample. Ultrapure water was added to the mold and frozen for 1h until it was completely frozen, and then the icicle was pushed at a constant speed with a thrust gauge. The peak force required to push down the icicle was recorded and its ice adhesion strength was calculated.

[0078] See also Figure 6 In order to verify the wear resistance of comparative examples 1 to 2, and to verify the durable cyclic performance of the micro-nano composite structure with high durability anti-icing effect, the samples were placed horizontally in a refrigerator at a temperature of -25°C and a relative humidity of 80%. A transparent uncovered square tube of 8mm×8mm×30mm was used as a mold and placed on the sample. Ultrapure water was added to the mold and frozen for 1h until completely frozen, and then the icicle was pushed at a constant speed with a thrust gauge to record the peak force required to push down the icicle. The period from the complete freezing of the icicle to the pushing down of the icicle was regarded as an icing and deicing cycle, and the ice adhesion strength after 50 icing and deicing cycles was recorded respectively.

[0079] Through the verification of the above-mentioned comparative examples 1 to 2 and embodiment 3, the micro-nano composite structure with high durability anti-icing effect provided by the present invention imitates the lotus leaf and pitcher plant structure through femtosecond laser and transfer, and its ice adhesion strength is much lower than that of comparative example 1 and comparative example 2, which is reduced by 83.1% compared with comparative example 1 and 89.9% compared with comparative example 2. After multiple icing and deicing cycles, the ice adhesion strengths of comparative examples 1 and 2 are close to 85 kPa and 165 kPa respectively, while the ice adhesion strength of embodiment 3 is still lower than 20 kPa. This shows that the present invention is not a simple superposition of the effects of the micro-column and micro-cone structure of comparative example 2 by injecting the liquid with reversible temperature response into the material of comparative example 1. The micro-nano composite structure provided by the present invention enables the droplets to maintain a stable Cassie-Baxter state even at low temperatures, reduces the ice adhesion strength, and achieves an ice-repellent effect; at the same time, when de-icing is not required at room temperature, the remaining lubricating liquid on the surface will be recovered to prevent the lubricating liquid from being lost; at the same time, the hydrophobicity of the surface will be improved, so that the microstructure will not be immersed in water to prevent ice from staying and being contaminated by dust. When de-icing is required at low temperatures, the internal lubricating liquid will be secreted to the surface of the structure to improve the ice-repellent property, and the internal lubricating liquid will also automatically replenish the surface to maintain a low ice adhesion strength, further improving durability.

[0080] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0081] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A laser processed micro-nano composite structure with anti-icing effect, characterized in that: include: A liquid injection surface with reversible temperature response is provided on the surface, wherein a microcolumn array is provided, wherein the microcolumn array includes a plurality of microcolumn structures arranged in a periodic array, wherein the top of each microcolumn structure is provided with a microcone array by laser processing, wherein the microcone array includes a plurality of microcone structures arranged in a periodic array.

2. The laser processed micro-nano composite structure with anti-icing effect as claimed in claim 1, characterized in that: The liquid-infused surface with reversible temperature response is a transparent and flexible surface.

3. The laser processed micro-nano composite structure with anti-icing effect as claimed in claim 1, characterized in that: The diameter of the microcone structure is 28-32 μm, and the center distance between the microcone structures is 28-32 μm; each of the microcolumn structures is distributed in a square shape, the height of the microcolumn structure is 380-400 μm, the diameter is 145-155 μm, and the distance between two adjacent microcolumn structures is 149-151 μm.

4. A method for preparing a laser-processed micro-nano composite structure with an anti-icing effect as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Using a femtosecond laser to process a plurality of through holes on a polytetrafluoroethylene sheet having a thickness of 400 μm, wherein each of the through holes is distributed in a square shape; S2, cleaning the processed polytetrafluoroethylene sheet in anhydrous ethanol for ten minutes and drying it to obtain a micro-column template; S3, spraying a release agent on the micro-column template obtained in S2, then pouring a liquid injection material with a reversible temperature response into the micro-column template to cover the micro-column template by 700-800 μm, and placing the micro-column template filled with the liquid injection material with a reversible temperature response into a drying oven at a temperature of 80-120° C. for curing for 1-4 hours and then demolding to obtain a micro-column array on the liquid injection surface with a reversible temperature response; S4. Use a femtosecond laser to scan the liquid injection surface with the microcolumn array obtained in S3. The incident direction of the laser beam is perpendicular to the liquid injection surface. Grid line scanning is performed on the surface of a single microcolumn structure. A microcone array is processed at the top of the microcolumn structure to obtain a micro-nano composite structure.

5. The method for preparing a laser-processed micro-nano composite structure with an anti-icing effect as claimed in claim 4, characterized in that: The material of the liquid-injected surface with reversible temperature response is polydimethylsiloxane doped with 60 wt % mixed lubricating liquid.

6. The method for preparing a laser-processed micro-nano composite structure with an anti-icing effect as claimed in claim 5, characterized in that: The lubricating liquid is prepared by mixing silicone oil and liquid paraffin in a mass ratio of 1:1, wherein the viscosity of the silicone oil is 100 mm 2 / s.

7. The method for preparing a laser-processed micro-nano composite structure with an anti-icing effect as claimed in claim 4, characterized in that: In S1, the diameter of the through holes is 145-155 μm, and the spacing is 149-151 μm.

8. The method for preparing a laser-processed micro-nano composite structure with an anti-icing effect as claimed in claim 4, characterized in that: In S4, the pulse energy of the femtosecond laser is 20-30 mW, and the scanning speed is 0.001 m·s -1 , the scanning grid line spacing is 28 to 32 μm.

9. An application of a laser-processed micro-nano composite structure with anti-icing effect as claimed in any one of claims 1 to 3, characterized in that: The micro-nano composite structure with high-durability anti-icing and deicing effect is applied in the field of anti-icing and deicing.

10. The application of the laser processed micro-nano composite structure with anti-icing effect as claimed in claim 9, characterized in that: The liquid injection surface with reversible temperature response is adhered to the surface of the required anti-icing and de-icing structure, and is used for anti-icing and de-icing on the surface of the required anti-icing and de-icing structure.