Impurity removal method of waste lithium iron phosphate and iron phosphate product
By baking and leaching waste lithium iron phosphate with (NH4)2SO4 and leaching water, the problem of difficult and high cost in recycling of waste lithium iron phosphate batteries is solved, efficient impurity removal and lithium leaching are achieved, and the The process of removing impurities reduces energy consumption and environmental pollution.
Patent Information
- Application Number
- CN202411195172.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
AI Technical Summary
The existing waste lithium iron phosphate battery recycling methods have problems such as complex recycling process, high cost, difficult to control impurities and environmental pollution, especially the high requirements for metal reuse and purity, and the existing methods cannot effectively reduce the loss of iron phosphate. .
The waste lithium iron phosphate is mixed with (NH4)2SO4 and then leaching with water. By adjusting the mass ratio, baking temperature and pH value, the effective removal of impurity elements (such as aluminum and calcium) and the efficient leaching of lithium are achieved. Simplify the removal process and reduce costs.
It has achieved impurities removal of waste lithium iron phosphate, efficient leaching of lithium, purification of iron phosphate, and simple process, environmentally friendly and low cost, reducing the high-temperature roasting process, reducing energy consumption and environmental pollution.
Smart Images

Figure CN118908166A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of impurity removal, and in particular to a method for removing impurities from waste lithium iron phosphate and an iron phosphate product. Background Art
[0002] With the continuous development of the new energy vehicle industry, my country will become the world's largest new energy vehicle market. Due to the short life of the batteries used, a large number of retired lithium iron phosphate batteries will appear in the future, and the number is showing a rapid growth trend. The harmful parts of retired lithium iron phosphate batteries will enter the environment and cause serious pollution. Recycling waste lithium iron phosphate batteries not only solves environmental problems, but also brings certain economic effects. In addition, the safety hazards such as fire and explosion caused by waste lithium iron phosphate should not be underestimated. Therefore, recycling waste lithium iron phosphate batteries is imminent.
[0003] At present, the recycling and treatment methods of waste lithium iron phosphate batteries mainly include hydrometallurgy, high-temperature solid phase recovery, bioleaching, pyrometallurgy, etc. Hydrometallurgy is widely used in the recycling and treatment of waste lithium iron phosphate batteries due to its advantages such as high metal recovery rate, easy process control, low energy consumption and less pollution, but it has disadvantages such as difficult to control the selectivity of recycled metals, small batch processing volume, and a lot of waste liquid. The high-temperature solid phase recovery process is relatively short, simple to operate, and does not require a large amount of acid and alkali reagents, but it has high requirements for the purity of the recycled raw materials, and the impurities therein will reduce the electrochemical properties of the resulting products. Although the bioleaching method is environmentally friendly and low in cost, it has the disadvantages of low leaching rate, high environmental requirements, and long cycle. Pyrometallurgy has the characteristics of wide application and high recovery rate, but the process not only has high energy consumption, but also produces a large amount of waste gas and other pollutants, and it is also impossible to effectively reuse various metals. It can be seen that the current recycling methods have the problems of complex recycling process and high cost. Summary of the invention
[0004] The purpose of this application is to provide a method for removing impurities from waste lithium iron phosphate to simplify the impurity removal process and reduce the cost of impurity removal. The specific technical solution is as follows:
[0005] A first aspect of the present application provides a method for removing impurities from waste lithium iron phosphate, wherein the waste lithium iron phosphate includes impurity elements, and the impurity elements include aluminum and / or calcium; the impurity removal method comprises the following steps:
[0006] (1) mixing the waste lithium iron phosphate with (NH4)2SO4, and then calcining to obtain a calcined product;
[0007] Wherein, the mass ratio X of the waste lithium iron phosphate and (NH4)2SO4 is 1:(0.6 to 1), the calcination temperature T1 is 250°C to 400°C, and the calcination time t1 is 0.5h to 12h;
[0008] (2) subjecting the roasted product to a slurry mixed with water and subjecting it to leaching treatment, filtering it to obtain a leachate and a filter residue, wherein the filter residue is a purified iron phosphate slag;
[0009] Wherein, the pH of the slurry is ≤3.
[0010] In some embodiments of the present application, in step (1), the mass ratio X is 1:(0.75 to 0.85).
[0011] In some embodiments of the present application, in step (1), the calcination temperature T1 is 300° C. to 350° C., and the calcination time t1 is 0.5 h to 4 h.
[0012] In some embodiments of the present application, in step (1), an oxygen-containing gas is continuously introduced during the roasting, and the oxygen-containing gas comprises air or oxygen.
[0013] In some embodiments of the present application, in step (1), before mixing (NH4)2SO4, it is ground and sieved, and the sieve has a mesh size of 50 to 200.
[0014] In some embodiments of the present application, in step (2), the solid-to-liquid ratio of the calcined product to water is 0.1 g / ml to 0.3 g / ml.
[0015] In some embodiments of the present application, in step (2), the pH of the slurry is 2≤pH≤3.
[0016] In some embodiments of the present application, in step (2), the temperature T2 of the leaching treatment is 15°C to 35°C, and the time t2 is 0.5h to 10h.
[0017] In some embodiments of the present application, in step (2), the leaching solution contains Li + and the impurity elements.
[0018] In some embodiments of the present application, the aluminum content in the filter residue is ≤500 ppm, and the calcium content is ≤100 ppm.
[0019] The second aspect of the present application provides an iron phosphate product, wherein the molar ratio of iron to phosphorus in the iron phosphate product is (0.96 to 1):1; the iron phosphate product is prepared from the purified iron phosphate slag obtained by the impurity removal method described in any of the preceding embodiments.
[0020] Beneficial effects of this application:
[0021] The present application provides a method for removing impurities from waste lithium iron phosphate, wherein the waste lithium iron phosphate includes impurity elements, and the impurity elements include aluminum and / or calcium; the impurity removal method comprises the following steps: (1) mixing the waste lithium iron phosphate with (NH4)2SO4, and then roasting, wherein the mass ratio X of the waste lithium iron phosphate to (NH4)2SO4 is 1:(0.6 to 1), and the roasting temperature T1 is 250°C to 400°C, and then the slurry obtained by mixing the roasted product with water is subjected to leaching treatment, filtered, and a leachate and a filter residue are obtained, wherein the filter residue is purified iron phosphate slag; wherein the pH of the slurry is ≤3. The impurity removal method provided by the present application can effectively remove the impurity elements in the waste lithium iron phosphate through roasting and leaching treatment, and coordinated regulation of the mass ratio X, the roasting temperature T1, and the pH of the slurry within the above range, and at the same time, Li + The leaching is efficient and the loss of iron phosphate is low. In addition, the impurity removal process of this process is simple, low-cost and environmentally friendly.
[0022] In the present application, waste lithium iron phosphate is decontaminated by roasting with (NH4)2SO4, carbon and organic matter can be removed, and the process of high-temperature roasting to remove carbon and organic matter is reduced (after low-temperature roasting at 250°C to 400°C, carbon and organic matter are removed by immersion in water), thus reducing the complicated decontamination process.
[0023] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.
[0025] Figure 1 It is the impurity removal flow chart in Example 1;
[0026] Figure 2 This is a photograph of the calcined product in Comparative Example 3. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.
[0028] A first aspect of the present application provides a method for removing impurities from waste lithium iron phosphate, wherein the waste lithium iron phosphate includes impurity elements, and the impurity elements include aluminum and / or calcium; the impurity removal method comprises the following steps:
[0029] (1) Mixing waste lithium iron phosphate with (NH4)2SO4, and then roasting to obtain a roasted product. The mass ratio X of waste lithium iron phosphate to (NH4)2SO4 is 1:(0.6 to 1), preferably, the mass ratio X is 1:(0.75 to 0.85); for example, the mass ratio X can be 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95 or 1:1, or between any two of the above ratios. The roasting temperature T1 is 250°C to 400°C, and the time t1 is 0.5h to 12h. Preferably, the roasting temperature T1 is 300°C to 350°C, and the time t1 is 0.5h to 4h. For example, T1 can be 250° C., 260° C., 270° C., 280° C., 290° C., 300° C., 310° C., 320° C., 330° C., 340° C., 350° C., 360° C., 370° C., 380° C., 390° C., or 400° C., or between any two of the above numbers. For example, t1 can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, or 12 h, or between any two of the above numbers. In this process, impurities (Al, Ca, etc.) in the waste iron phosphate as well as organic matter and carbon are removed by roasting the waste lithium iron phosphate with (NH4)2SO4, that is, only the roasting method is used, which is conducive to the subsequent realization of the purpose of Li leaching and impurity removal.
[0030] (2) The slurry obtained by mixing the calcined product with water is subjected to leaching treatment and filtered to obtain a leachate and a filter residue, wherein the filter residue is a purified iron phosphate slag. The pH of the slurry is ≤3, and preferably, the pH of the slurry is 2≤pH≤3. For example, the pH of the slurry can be 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3, or between any two of the above numbers. In this process, Li is achieved by water leaching. + The separation of impurity elements and iron phosphate is novel and less water is used during water immersion.
[0031] The present application does not particularly limit the source of waste lithium iron phosphate. For example, waste lithium iron phosphate batteries are disassembled to obtain positive electrodes, and the positive electrode current collector and the positive electrode material layer of the disassembled positive electrode are separated. The obtained positive electrode material layer is also waste lithium iron phosphate, and the waste lithium iron phosphate may include but is not limited to lithium iron phosphate, organic matter, carbon, etc. The present application does not limit the above-mentioned organic matter and carbon. For example, the organic matter can be a binder in the positive electrode material layer, and the carbon can be a conductive agent in the positive electrode material layer.
[0032] The impurity removal method provided by the present application, through roasting, the impurity elements in the waste lithium iron phosphate react with (NH4)2SO4 to generate sulfates of impurity elements, and the iron and lithium elements in the waste lithium iron phosphate react with (NH4)2SO4 to generate iron phosphate and lithium sulfate, and organic matter and carbon in the waste lithium iron phosphate can also be removed. Subsequently, the roasted product after roasting is leached with water. Since the sulfates of the impurity elements are soluble in water or slightly soluble in water, and iron phosphate is insoluble in water, the leaching treatment is followed by filtration, and iron phosphate can be separated from the impurity elements; at the same time, lithium sulfate is soluble in water, and the separation of lithium elements is also achieved by leaching. Thus, the impurity removal method provided by the present application can obtain purified iron phosphate slag only by roasting, leaching treatment, and filtration, the impurity removal process is simple, and the (NH4)2SO4 used is cheap, which can reduce the cost of impurity removal; and no alkali is used in the impurity removal process, which can further reduce the cost of impurity removal, and at the same time, lithium leaching and removal of impurity elements by water leaching are more environmentally friendly. That is, the impurity removal method provided in the present application is not only simple in process and low in cost, but also environmentally friendly.
[0033] In step (1), waste lithium iron phosphate and (NH4)2SO4 are mixed in a mass ratio (waste lithium iron phosphate: (NH4)2SO4=1:0.6-1) and then roasted. The mass ratio of waste lithium iron phosphate to (NH4)2SO4 is in the range of 1:0.6-1, which is conducive to the subsequent realization of efficient lithium leaching rate and low iron phosphate loss (lithium leaching rate is above 90%, and iron phosphate loss is within 10wt%), and ensures the effective leaching of other impurity elements (Al, Ca, etc.).
[0034] Further preferably, the mass ratio of waste lithium iron phosphate to (NH4)2SO4 is 1:(0.75 to 0.85), which can further achieve lithium leaching filtration of more than 99% and iron phosphate loss within 6wt%.
[0035] In step (1), when the mass ratio X of waste lithium iron phosphate to (NH4)2SO4 is too small, for example, less than 1:0.6 (such as 1:0.4, 1:0.3 ... etc.), the leaching rate of lithium in step (2) is reduced; when the mass ratio X of waste lithium iron phosphate to (NH4)2SO4 is too large, for example, greater than 1:1 (such as 1:1.1, 1:1.2 ... etc.), the excess (NH4)2SO4 will cause the Fe element in the waste lithium iron phosphate to be converted into Fe2(SO4)3, thereby increasing the loss of iron phosphate. Therefore, by regulating the mass ratio X of waste lithium iron phosphate to (NH4)2SO4 within the above range, it is not easy to lose iron phosphate, which is conducive to obtaining more purified iron phosphate slag, and the leaching rate of lithium element is high.
[0036] During the roasting process, if the temperature T1 is too high, for example, higher than 400°C, the waste lithium iron phosphate is easily oxidized into iron oxide, which increases the loss of iron phosphate. More importantly, by adjusting the temperature T1 within the above range, (NH4)2SO4 is liquid, and the pH is acidic, and it can react with organic matter and carbon in the waste lithium iron phosphate at temperature T1, thereby removing organic matter and carbon, avoiding high-temperature roasting to remove carbon and organic matter, and reducing energy consumption. By adjusting the temperature T1 during roasting within the above range, the waste lithium iron phosphate and (NH4)2SO4 can fully react, which is conducive to the impurity elements and lithium elements to form corresponding sulfates, and the iron element to form iron phosphate, and the iron element is not easily oxidized into iron oxide, thereby achieving effective separation of iron phosphate and impurity elements in step (2), and sufficient leaching of lithium elements.
[0037] In step (2), after the above-mentioned roasted product is cooled to room temperature, it is put into water for Li leaching (the amount of water should not be too much, pH ≤ 3), and filtered and dried after Li leaching. When the pH is lower than 3, the aluminum element will exist in the form of ions; when the pH of the slurry is too high, for example, greater than 3, Al(OH)3 precipitation is easily generated, which will exist in the purified iron phosphate slag after leaching treatment and filtration, affecting its purity. When the pH of the slurry is too low, the iron phosphate may dissolve in the liquid phase again. By adding water to adjust the pH of the slurry within the above range, the aluminum element exists in the form of ions, and after leaching treatment and filtration, it mainly exists in the leachate, which can achieve effective separation from the iron phosphate and improve the purity of the purified iron phosphate slag.
[0038] In this process, the amount of (NH4)2SO4, the roasting temperature and the pH of lithium leaching with water can significantly affect the content of impurities in the crystalline iron phosphate, the lithium leaching effect and the loss of iron phosphate. In summary, the impurity removal method provided by the present application can effectively remove the impurity elements in the waste lithium iron phosphate by roasting with ammonium sulfate, leaching with water, and regulating the mass ratio X, roasting temperature T1, and pH of the slurry within the above range, and efficiently leaching lithium, and the impurity removal process is simple, low-cost, and environmentally friendly.
[0039] In some embodiments of the present application, in step (1), an oxygen-containing gas is continuously introduced during roasting, and the oxygen-containing gas includes air or oxygen. The aluminum on the surface of waste lithium iron phosphate usually exists in the form of oxide, and there may also be some aluminum element inside. The oxygen-containing gas is continuously introduced during roasting, which can convert the internal aluminum element into aluminum oxide, thereby facilitating the reaction with (NH4)2SO4 to form aluminum sulfate. The present application has no particular restrictions on the flow rate of the oxygen-containing gas, as long as the purpose of the present application can be achieved. Exemplarily, the flow rate of the oxygen-containing gas can be 24L / min to 36L / min. In the oxygen-containing gas, the volume content of oxygen is greater than or equal to 15%.
[0040] In some embodiments of the present application, step (1) includes the following reaction:
[0041] Al2O3+3(NH4)2SO4=Al2(SO4)3+6NH3+3H2O;
[0042] CaO+(NH4)2SO4=CaSO4+2NH3+H2O;
[0043] 4LiFePO4+2(NH4)2SO4+O2=4FePO4+2Li2SO4+4NH3+2H2O.
[0044] Among them, Al2(SO4)3 is soluble in water. After the roasting reaction, the Al element in the waste can be efficiently leached; CaSO4 is slightly soluble in water, with a solubility of about 0.2g / 100ml. Since the Ca content in the waste is not much, even if CaSO4 is slightly soluble in water after the reaction, most of the Ca elements can be effectively leached, so that the Ca content in the obtained iron phosphate slag meets the requirements; Li2SO4 is soluble in water, and FePO4 is insoluble in water. After leaching treatment, the impurity elements aluminum and calcium can be separated from the iron phosphate, and the leaching of lithium can be achieved.
[0045] In some embodiments of the present application, in step (1), before mixing (NH4)2SO4, grinding and sieving are performed, and the sieve is 50 mesh to 200 mesh. For example, the sieve can be 50 mesh, 60 mesh, 70 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 170 mesh or 200 mesh. Before mixing (NH4)2SO4 with waste iron phosphate, grinding and sieving are performed, which is conducive to fully mixing (NH4)2SO4 with waste iron phosphate, so that they can fully react during the roasting process.
[0046] In some embodiments of the present application, in step (2), the solid-to-liquid ratio Y of the roasted product to water is 0.1g / ml to 0.3g / ml. For example, the solid-to-liquid ratio Y can be 0.1g / ml, 0.11g / ml, 0.12g / ml, 0.13g / ml, 0.14g / ml, 0.15g / ml, 0.16g / ml, 0.17g / ml, 0.18g / ml, 0.19g / ml, 0.2g / ml, 0.21g / ml, 0.22g / ml, 0.23g / ml, 0.24g / ml, 0.25g / ml, 0.26g / ml, 0.27g / ml, 0.28g / ml, 0.29g / ml or 0.3g / ml, or between any two of the above-mentioned numbers. Al2(SO4)3 has a higher solubility in water, and CaSO4 has a lower solubility in water than Al2(SO4)3. By adjusting the solid-liquid ratio Y within the above range, during the leaching process, CaSO4 and Al2(SO4)3 can be fully dissolved in water, which is beneficial to achieve effective separation of iron phosphate and impurity elements and improve the purity of purified iron phosphate slag.
[0047] In some embodiments of the present application, in step (2), the temperature T2 of the leaching treatment is 15°C to 35°C, and the time t2 is 0.5h to 10h. For example, T2 can be 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C or 35°C, or between any two of the above numbers. For example, t2 can be 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h, or between any two of the above numbers. By regulating the temperature T2 and time t2 of the leaching treatment within the above range, CaSO4 and Al2(SO4)3 can be fully dissolved in water, which is beneficial to achieve effective separation of iron phosphate and impurity elements, improve the purity of purified iron phosphate slag, and reduce energy consumption.
[0048] In some embodiments of the present application, in step (2), the leaching solution contains Li + and impurity elements. Li can be further separated + With impurities Al and Ca elements, for example, by adjusting the pH with alkali solution, precipitating Al and Ca elements, and mixing them with Li + The present application does not limit the above-mentioned alkali solution, as long as the purpose of the present application can be achieved.
[0049] In some embodiments of the present application, the aluminum content W1 in the filter residue is ≤500ppm, and the calcium content W2 is ≤100ppm. For example, W1 can be 5ppm, 10ppm, 20ppm, 30ppm, 50ppm, 70ppm, 90ppm, 100ppm, 150ppm, 200ppm, 250ppm, 300ppm, 350ppm, 400ppm, 450ppm or 500ppm, or between any two of the above numbers. For example, the mass ratio X can be 5ppm, 10ppm, 20ppm, 30ppm, 40ppm, 50ppm, 60ppm, 70ppm, 80ppm, 90ppm or 100ppm, or between any two of the above numbers. The aluminum content and calcium content in the filter residue are within the above range, indicating that the impurity element content in the filter residue is very small, and the purity of the purified iron phosphate slag obtained is high.
[0050] In some embodiments of the present application, in step (2), the filter residue obtained is further dried to obtain purified iron phosphate residue. The present application does not limit the drying parameters, as long as the purpose of the present application can be achieved.
[0051] The second aspect of the present application provides an iron phosphate product, wherein the molar ratio Z of iron to phosphorus in the iron phosphate product is (0.96 to 1):1; for example, the molar ratio Z can be 0.96:1, 0.97:1, 0.98:1, 0.99:1 or 1:1, or between any two of the above numbers. The iron phosphate product is prepared from the purified iron phosphate slag obtained by the impurity removal method in any of the aforementioned embodiments, that is, the molar ratio of iron to phosphorus in the purified iron phosphate slag obtained by the impurity removal method provided by the present application is (0.96 to 1):1, which meets the standard and can be used to prepare lithium iron phosphate, a positive electrode material of secondary battery materials, thereby realizing the recycling and reuse of waste lithium iron phosphate materials.
[0052] In some embodiments of the present application, the preparation steps of preparing the ferrous phosphate product from the purified ferrous phosphate slag may include but are not limited to the following steps: the purified ferrous phosphate slag is subjected to acid dissolution, water mixing, and crystallization to obtain the ferrous phosphate product. The present application does not limit the specific steps of the above-mentioned acid dissolution, water mixing, and crystallization, as long as the desired ferrous phosphate product can be obtained. Exemplarily, the acid used for acid dissolution may include but is not limited to at least one of phosphoric acid, hydrochloric acid, and sulfuric acid.
[0053] Example
[0054] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.
[0055] Example 1 (the mass ratio of waste lithium iron phosphate to ammonium sulfate is 1:0.8)
[0056] Figure 1 The experimental flow chart of Example 1 is as follows:
[0057] Take 3g of waste lithium iron phosphate and 2.4g of ammonium sulfate (mass ratio of 1:0.8) and mix them. Before mixing, grind the ammonium sulfate and pass it through a 200-mesh sieve. After mixing, continue to ventilate at T1=300℃ for t1=0.5h. After calcination, put the calcined material into water according to the solid-liquid ratio of 0.3g / ml. After mixing, the slurry pH=2.2, and then carry out leaching treatment, that is, leaching Li and removing impurities. The lithium leaching temperature T2 is 25℃, and the time t2 is 0.5h. After completion, filter to obtain the leachate and filter residue. After drying the filter residue, 2.85g of filter residue (the loss of iron phosphate is 5wt%) is obtained. The filter residue is subjected to inductively coupled plasma mass spectrometry (ICP) detection. The Li leaching rate is 99.8%. After lithium leaching, the Al content in the filter residue is 300ppm and the Ca content is 80ppm.
[0058] During the lithium immersion process after calcination, no carbon powder was found floating on the water surface, indicating that the carbon in the waste lithium iron phosphate was removed, and the calcined product was completely infiltrated with water, indicating that the organic matter in the waste lithium iron phosphate was removed.
[0059] Among them, the loss of iron phosphate = (1-mass of filter residue / waste lithium iron phosphate) × 100%; Li leaching rate = lithium content in leachate / lithium content in waste lithium iron phosphate × 100% (the same applies to other embodiments).
[0060] Table 1 Content of each element in waste lithium iron phosphate (before impurity removal)
[0061]
[0062]
[0063] As can be seen from the table above, waste lithium iron phosphate contains high levels of Al and Ca impurities. Using it in the preparation of products will result in too high an impurity content in the final product, which does not meet product requirements. Therefore, waste lithium iron phosphate needs to be decontaminated. When waste lithium iron phosphate is roasted with ammonium sulfate, the Ca impurities therein are converted into calcium sulfate. According to the solubility of calcium sulfate, it can be completely dissolved during leaching. Al impurities are eventually converted into aluminum sulfate. When the pH of the water leaching solution is not higher than 3, it will be completely dissolved, thereby achieving the separation of iron phosphate and impurity elements.
[0064] Example 2 (the mass ratio of waste lithium iron phosphate to ammonium sulfate is 1:0.6)
[0065] The only difference from Example 1 is that the mass ratio of waste lithium iron phosphate to ammonium sulfate is regulated, and the rest is the same as Example 1, specifically as follows:
[0066] Mix 3 g of waste lithium iron phosphate and 1.8 g of ammonium sulfate.
[0067] In this embodiment, the Li leaching rate is 90.6%. After leaching, filtering and drying, 2.83 g of filter residue is obtained (the loss of iron phosphate is 5.6 wt%). The Al content in the filter residue is 400 ppm and the Ca content is 90 ppm.
[0068] By comparing Example 2 with Example 1, it can be seen that when the mass ratio of waste lithium iron phosphate to ammonium sulfate is adjusted from 1:0.6 to 1:0.8, the impact on the loss of iron phosphate and the content of impurities Al and Ca in the filter residue is small, but the lithium leaching rate can be improved.
[0069] Example 3 (the mass ratio of waste lithium iron phosphate to ammonium sulfate is 1:1)
[0070] The only difference from Example 1 is that the mass ratio of waste lithium iron phosphate to ammonium sulfate is regulated, and the rest is the same as Example 1, specifically as follows:
[0071] Mix 3 g of waste lithium iron phosphate and 3 g of ammonium sulfate.
[0072] In this embodiment, the Li leaching rate is 99.0%. After leaching, filtering and drying, 2.76 g of filter residue is obtained (the loss of iron phosphate is 8 wt%). The Al content in the filter residue is 450 ppm and the Ca content is 50 ppm.
[0073] By comparing Example 3 with Example 1, it can be seen that when the mass ratio of waste lithium iron phosphate to ammonium sulfate is adjusted from 1:1 to 1:0.8, the effect on the leaching rate of lithium and the content of impurities Al and Ca in the filter residue is small, but the loss of iron phosphate can be reduced.
[0074] Embodiment 4 to Embodiment 7
[0075] The parameter changes are shown in Table 2, and the rest are the same as in Example 1.
[0076] Example 4 is similar to Example 1, except that the roasting temperature is adjusted to 350°C. From the experimental results, it can be seen that the effect is similar to that of Example 1, indicating that a roasting temperature of 300°C to 350°C can obtain a better impurity removal effect and a high lithium leaching rate, and the loss of iron phosphate is low.
[0077] Example 5 adjusts the roasting time and the solid-liquid ratio of water added after roasting on the basis of Example 4. It can be seen that when the roasting time is 0.5h to 4h and the solid-liquid ratio is in the range of 0.1g / ml0.3g / ml, good impurity removal effect and high lithium leaching rate can be obtained, and the loss of iron phosphate is also low.
[0078] Example 6 is similar to Example 1, except that the calcination temperature is further increased to 400°C. In Example 6, due to the high calcination temperature, ammonium sulfate volatilizes faster and has no time to react with the waste lithium iron phosphate. Therefore, the lithium immersion effect and the impurity removal effect are worse than those in Example 1. As for the loss of iron phosphate, since the filter residue will also contain a small amount of unreacted waste lithium iron phosphate, it will affect the calculation of the loss of iron phosphate.
[0079] Example 7 is similar to Example 1, except that the roasting time is increased (12 h), and the solid-liquid ratio of water added after roasting is adjusted to 0.2 g / ml. Good impurity removal effect and high lithium leaching rate can still be obtained, and the loss of iron phosphate is low.
[0080] Comparative Example 1 (the mass ratio of waste lithium iron phosphate to ammonium sulfate is 1:0.4)
[0081] The only difference from Example 1 is that 3 g of waste lithium iron phosphate is mixed with 1.2 g of ammonium sulfate (mass ratio is 1:0.4), and the rest is the same as Example 1.
[0082] 2.80 g of filter residue was obtained, and the loss of iron phosphate was 6.7 wt %. ICP test was performed on the filter residue, and the Li leaching rate was 71%.
[0083] It can be seen that compared with Example 1, when the mass ratio of lithium iron phosphate to ammonium sulfate is 1:0.4, Comparative Example 1 has a smaller effect on the loss of iron phosphate and a greater effect on the Li leaching rate, which is reduced to 71.0%.
[0084] Comparative Example 2 (the mass ratio of waste lithium iron phosphate to ammonium sulfate is 1:1.1)
[0085] The only difference from Example 1 is that 3 g of waste lithium iron phosphate is mixed with 3.3 g of ammonium sulfate (mass ratio is 1:1.1), and the rest is the same as Example 1.
[0086] 2.7 g of filter residue was obtained, and the loss of iron phosphate was 10 wt %. The filter residue was tested by ICP, and the Li leaching rate was 99%.
[0087] When there is too much ammonium sulfate, ammonium sulfate and ferric phosphate react as follows:
[0088] 2FePO4+3(NH4)2SO4=Fe2(SO4)3+2(NH4)3PO4.
[0089] It can be seen that compared with Example 1, in Comparative Example 2, the excess (NH4)2SO4 will cause the Fe element in LFP to be converted into Fe2(SO4)3, the loss of iron phosphate will increase, and the effect on the Li leaching rate will be small.
[0090] Comparative Example 3 (the calcination temperature is too high, 500°C, LFP will be oxidized into red iron oxide)
[0091] The difference from Example 1 is that the calcination temperature is 500°C, and the rest is the same as Example 1. After calcination, it is found that part of the lithium iron phosphate is oxidized into red iron oxide, such as Figure 2 As shown, no subsequent operations can be performed.
[0092] Comparative Example 4
[0093] The difference from Example 1 is that the solid-liquid ratio of water added after roasting is 0.05g / ml, and the pH of the slurry after mixing is 3.1. During the water adding process, white precipitate Al(OH)3 is found to be produced, which will affect the purity of the solid phase iron phosphate and the impurity removal efficiency is low.
[0094] The preparation parameters and performance tests of each embodiment and comparative example are shown in Table 2.
[0095] Table 2
[0096]
[0097] Note: " / " in Table 2 indicates that there is no corresponding parameter or performance; the Li leaching rate in Comparative Example 1 is too low, and the iron phosphate loss in Comparative Example 2 is too large, so the final impurity content is not tested; the subsequent operation in Comparative Example 3 cannot be carried out, and the iron phosphate loss, Li leaching rate and impurity content cannot be tested; other precipitation is generated in Comparative Example 4, so the iron phosphate loss, Li leaching rate and impurity content are not tested.
[0098] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A method for removing impurities from waste lithium iron phosphate, wherein: The waste lithium iron phosphate contains impurity elements, and the impurity elements include aluminum and / or calcium; the impurity removal method comprises the following steps: (1) mixing the waste lithium iron phosphate with (NH4)2SO4, and then calcining to obtain a calcined product; Wherein, the mass ratio X of the waste lithium iron phosphate and (NH4)2SO4 is 1:(0.6 to 1), the calcination temperature T1 is 250°C to 400°C, and the calcination time t1 is 0.5h to 12h; (2) subjecting the roasted product to a slurry mixed with water and subjecting it to leaching treatment, filtering it to obtain a leachate and a filter residue, wherein the filter residue is a purified iron phosphate slag; Wherein, the pH of the slurry is ≤3.
2. The impurity removal method according to claim 1, wherein: In step (1), the mass ratio X is 1:(0.75 to 0.85).
3. The impurity removal method according to claim 1, wherein: In step (1), the calcination temperature T1 is 300° C. to 350° C., and the calcination time t1 is 0.5 h to 4 h.
4. The impurity removal method according to claim 1, wherein: In step (1), oxygen-containing gas is continuously introduced during the roasting, and the oxygen-containing gas comprises air or oxygen.
5. The impurity removal method according to claim 1, wherein: In step (2), the solid-to-liquid ratio of the calcined product to water is 0.1 g / ml to 0.3 g / ml.
6. The impurity removal method according to claim 1, wherein: In step (2), the pH value of the slurry is 2≤pH≤3.
7. The impurity removal method according to claim 1, wherein: In step (2), the leaching treatment temperature T2 is 15°C to 35°C, and the time t2 is 0.5h to 10h.
8. The impurity removal method according to claim 1, wherein: In step (2), the leaching solution contains Li + and the impurity elements.
9. The impurity removal method according to claim 1, wherein: The aluminum content in the filter residue is ≤500ppm, and the calcium content is ≤100ppm.
10. An iron phosphate product, wherein: The molar ratio of iron to phosphorus in the ferric phosphate product is (0.96 to 1):1; The ferric phosphate product is prepared from the purified ferric phosphate slag obtained by the impurity removal method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for recycling waste lithium iron phosphate battery at low temperature regenerating lithium iron phosphate positive electrode material
CN113562717A
Purification treatment method and system for ferrophosphorus slag mixture containing Al and Cu impurities
CN114421044A
Method for extracting lithium from amblygonite and preparing iron-containing phosphate