Composite polyanion powder material as well as preparation method and application thereof
Through one-step mixing method and spray drying technology combined with seed crystal induced method, the problems of long drying cycle and poor conductivity in the synthesis of polyanionic powder materials were solved, and a composite polyanionic powder material with uniform size and high purity was prepared, which significantly Improved battery performance.
Patent Information
- Application Number
- CN202410958121.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing synthesis methods of polyanionic powder materials have problems such as long drying cycle, large energy consumption, use of toxic and harmful epoxides, complex operation and difficult to prepare in large-scale batches, resulting in poor conductivity and poor performance of the materials.
Precursor mixture is prepared by a one-step mixing method, using the combination of organic carbon and inorganic carbon to form uniformly coated particles during spray drying, and the seed crystals are induced to form a composite polyanionic powder material of uniform size, and through step-by-step sintering The composite polyanionic powder material was obtained by crushing with air flow.
It realizes rapid synthesis, single crystal structure, high purity and uniform size composite polyanionic powder materials, which improves battery performance, especially at a rate of 0.1C and has high specific capacity and excellent cycle stability.
Smart Images

Figure CN118908177A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery material synthesis, and in particular to a composite polyanion powder material and a preparation method and application thereof. Background Art
[0002] At present, the main methods for synthesizing polyanion powder materials in the industry are solid-phase reaction and sol-gel method. Chinese patent CN102468481B discloses a method for preparing polyanion positive electrode materials for lithium-ion batteries. The raw material precursors are mixed and dried by sol-gel method and then calcined to synthesize. The precursor material is obtained by adding an organic epoxy compound to initiate gelation during the sol-gel process. The polyanion positive electrode material prepared by this preparation method has the advantages of small particle size, uniform distribution, and large specific surface area. However, there are several disadvantages in this preparation method: (1) The drying cycle is long and the energy consumption of the drying process is high. (2) The use of toxic and harmful epoxides as initiators makes post-processing difficult and does not conform to the green and environmentally friendly production concept; (3) The operation is complicated and it is difficult to prepare in large quantities. Chinese patent CN115881948A discloses a method for preparing polyanion powder materials by solid-phase synthesis reaction. The precursor material is pre-sintered and then mixed with a carbon source and sintered again to prepare a modified polyanion material. This preparation method has complicated steps, long reaction time, and the preparation process will form mixed crystals, which are not uniform in crystal form. In addition, the polyanion material prepared by this preparation method has poor conductivity, resulting in poor performance in batteries.
[0003] Therefore, at this stage, there is an urgent need for a composite polyanion powder material that can be quickly synthesized, has a single crystal structure, few pure crystal defects, uniform size, and excellent battery performance. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide a composite polyanion powder material and its preparation method and application. A precursor mixture is prepared by a one-step mixing method, and the combination of organic carbon and inorganic carbon is used to promote the formation of uniformly coated particles during the spray drying process; seed crystals are used to induce the precursor mixture to form a composite polyanion powder material of uniform size.
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a composite polyanion powder material, which specifically comprises the following steps:
[0006] S1. Mixing a precursor source, a dispersant, an organic carbon source, an inorganic carbon source, a seed crystal, and a solvent to form a precursor mixture; the precursor source includes a sodium source, a transition metal source, and an anion source; the seed crystal has the same crystal form as the polyanion material in the composite polyanion powder material; and the mass ratio of the organic carbon source and the inorganic carbon source to the precursor source is 5-10 wt %;
[0007] S2. removing the solvent from the precursor mixture in S1 by spray drying technology to obtain a precursor intermediate;
[0008] S3. The precursor intermediate described in step S2 is sequentially subjected to step-by-step sintering, airflow pulverization, and demagnetization under an inert gas environment to obtain the composite polyanion powder material.
[0009] Furthermore, in step S1, the mass ratio of the seed crystal to the precursor source in the precursor mixture is 1-5:100.
[0010] Furthermore, in step S1, the seed crystal has a particle size of 0.01-2 μm; the seed crystal is prepared by pressure sintering, and the preparation method is as follows:
[0011] A precursor source, a dispersant and a solvent are mixed to form a seed crystal mixture; the solvent in the seed crystal mixture is removed by spray drying technology to obtain a seed crystal precursor intermediate; the seed crystal precursor intermediate is prepared into a ceramic blank by static pressing, and the seed crystal is obtained after high-temperature sintering and crushing.
[0012] Furthermore, in the seed crystal treatment step: the static pressure is 100-200 MPa; and the high temperature sintering temperature is 600-900°C.
[0013] The seed crystals are produced through a pressurized sintering process, performed at a higher temperature than that of standard materials and with a longer hold time to promote grain growth. Ceramic sintering theory indicates that each grain is a single crystal with minimal lattice defects. No inorganic or organic carbon sources are added during the seed crystal preparation process, and grain growth is limited only by the kinetics of sintering temperature and time, not by the physical constraints of carbon coating. Therefore, the grains grow very easily, with a primary particle size of 200-800 microns. The seed crystal particle size is controlled by pulverization. Only by keeping the seed crystals within a small particle size range can the particle size of the seed-induced composite polyanion powder material be controlled within a range of 5-20 μm.
[0014] Furthermore, in step S1, the inorganic carbon source is selected from one or more of acetylene black, Ketjen black, graphite, activated carbon and carbon nanospheres;
[0015] The organic carbon source is selected from one or more of glucose, sucrose, starch, polyethylene glycol, polyvinyl alcohol, polyacrylic acid and citric acid.
[0016] Furthermore, in step S1, the mixing is ball milling mixing, the ball milling speed is 100-500 r / min, the ball milling beads are made of zirconia, the diameter of the ball milling beads is 3-10 mm, and the ball milling time is 2-6 h; the solid content of the mixture is 20-60 wt%.
[0017] Furthermore, in the spray drying step in step S2, the inlet air temperature range is 180-240°C, the outlet air temperature range is 90-120°C, and the centrifugal speed range is 25000-35000 r / min.
[0018] Furthermore, the step-by-step sintering process in step S3 includes a first sintering step and a second sintering step: the first sintering step has a heating rate of 1-10°C / min, a sintering temperature of 300-400°C, and a holding time of 1-5h;
[0019] In the second step of sintering treatment, the sintering temperature is 450-800°C and the holding time is 2-5h;
[0020] The flow rate of the inert gas is 10-300 ml / min; the purity of the inert gas is not less than 99.99%.
[0021] The second aspect of the present invention further provides a composite polyanion powder material, which is prepared by the preparation method described in the first aspect; the composite polyanion powder material comprises a polyanion material and a carbon material.
[0022] The third aspect of the present invention is to provide a battery pole piece, comprising the composite polyanion powder material described in the second aspect.
[0023] A fourth aspect of the present invention is to provide a sodium ion battery, which includes the electrode plate described in the third aspect.
[0024] Beneficial effects of the present invention:
[0025] The present invention utilizes a simple method for preparing a composite polyanion powder material. A uniformly coated polyanion material is obtained through a one-step process to prepare a precursor mixture. Seed crystals are added as precursors to the mixing process to coat the polyanion powder surface and instantaneously dry and granulate it. This effectively controls the reaction morphology and induces crystal growth and diffusion pathways, resulting in a uniformly sized composite polyanion powder material. Compared to solid-phase reactions, this method can reduce the sintering and holding time to just 3 hours, enabling continuous production of polyanion materials with specific crystal forms, thus possessing high industrial application value.
[0026] 2. The organic carbon source is soluble in the solvent, allowing it to be better coated on the powder surface, improving the powder's conductivity. During the spray drying process, powder materials tend to stick together, making it difficult to effectively control the material's morphology. The inorganic carbon used in this invention is insoluble in the precursor solvent. During the spray drying process, it effectively isolates the powder, inhibiting abnormal seed-induced crystal growth. The resulting crystals are higher in purity and have fewer defects. Furthermore, it improves the powder's conductivity.
[0027] 3. The battery prepared using the polyanion powder material of the present invention has a very high specific capacity (100-120 mAh / g) at a rate of 0.1C and exhibits excellent cycle stability (the capacity retention rate of 1200 cycles at a rate of 1C is 98.7%). BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a diagram showing the mechanism of seed crystal induction crystal formation according to the present invention;
[0029] Figure 2 This is a scanning electron microscope (SEM) image of the composite polyanion powder material prepared in Example 2 of the present invention;
[0030] Figure 3 This is a scanning electron microscope (SEM) image of the composite polyanion powder material prepared in Comparative Example 2 of the present invention;
[0031] Figure 4 1 is the X-ray diffraction pattern (XRD) of the composite polyanion powder material prepared in Example 1 and Comparative Example 1 of the present invention;
[0032] Figure 5 2 is the X-ray diffraction pattern (XRD) of the composite polyanion powder material prepared in Example 2 of the present invention and Comparative Example 2;
[0033] Figure 6 The cycle performance of the composite polyanion powder materials prepared in Example 1 and Comparative Example 1 of the present invention when assembled into batteries;
[0034] Figure 7 The graph shows the cycle performance of the composite polyanion powder materials prepared in Example 2 of the present invention and Comparative Example 2 when assembled into batteries. DETAILED DESCRIPTION
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention pertains. The terms used herein in the specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the relevant listed items. The term "includes" or "comprising" described in the present invention means that in addition to the components described, it may also include or contain other components. The term "includes" or "comprising" described in the present invention may also be replaced by the closed form "for" or "consisting of..."
[0036] As described in the background art, currently, conventional solid-phase reactions cannot achieve large-scale preparation of polyanionic materials. Furthermore, the preparation process consumes a lot of energy, and the morphology and purity of the crystals cannot be effectively controlled. This greatly limits the practical application of polyanionic materials.
[0037] To solve the above problems, an embodiment of the present invention provides a method for preparing a composite polyanion powder material, comprising the following steps:
[0038] S1. Mixing a precursor source, a dispersant, an organic carbon source, an inorganic carbon source, a seed crystal, and a solvent to form a precursor mixture; the precursor source includes a sodium source, a transition metal source, and an anion source; the seed crystal has the same crystal form as the polyanion material in the composite polyanion powder material; and the mass ratio of the organic carbon source and the inorganic carbon source to the precursor source is 5-10 wt %;
[0039] S2. removing the solvent from the precursor mixture in S1 by spray drying technology to obtain a precursor intermediate;
[0040] S3. The precursor intermediate described in step S2 is sequentially subjected to step-by-step sintering, airflow pulverization, and demagnetization under an inert gas environment to obtain the composite polyanion powder material.
[0041] In some preferred embodiments, the mass ratio of the seed crystal to the precursor source in the precursor mixture is 1-5:100; for example, 1:100, 2:100, 3:100, 4:100, 5:100, etc., including but not limited to the ratios listed above.
[0042] In some preferred embodiments, the inorganic carbon source is selected from one or more of acetylene black, Ketjen black, artificial graphite, natural graphite, carbon fiber, carbon nanotube dry powder and graphene; the organic carbon source is selected from one or more of glucose, sucrose, starch, polyethylene glycol, polyvinyl alcohol, polyacrylic acid and citric acid.
[0043] During the spray drying process, the precursor mixture dries rapidly to form larger particles, causing adhesion between the polyanion powders and, in turn, uneven carbon coating on their surfaces, affecting the electrochemical performance of the battery. In this embodiment, the organic carbon in the precursor mixture is soluble in the solvent, forming a uniform coating on the surface of the precursor powder. Because the inorganic carbon is insoluble in the solvent, it acts as a barrier to separate the powder particles during the spray drying process and inhibits abnormal crystal growth caused by the presence of seed crystals.
[0044] In some preferred embodiments, the dispersant is an inorganic alkali metal phosphate and / or an organic polymer; preferably, it is selected from one or more of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, polyacrylic acid, polyvinyl alcohol, and polyethylene glycol; more preferably, polyacrylic acid. The dispersant accounts for 0.1-2 wt% of the precursor source, preferably 2 wt%.
[0045] In some preferred embodiments, the mixing is ball milling, the ball milling speed is 100-500 r / min, the ball milling beads are made of zirconia, the diameter of the ball milling beads is 3-10 mm, and the ball milling time is 2-6 h; the solid content of the mixture is 20-60 wt%.
[0046] In some preferred embodiments, the seed crystal has a particle size of 0.01-2 μm; the seed crystal is prepared by pressure sintering, and the preparation method is as follows:
[0047] A precursor source, a dispersant and a solvent are mixed to form a seed crystal mixture; the solvent in the seed crystal mixture is removed by spray drying technology to obtain a seed crystal precursor intermediate; the seed crystal precursor intermediate is prepared into a ceramic blank by static pressing, and the seed crystal is obtained after high-temperature sintering and crushing.
[0048] Preferably, in the seed crystal treatment step: the static pressure is 100-200 MPa; and the high-temperature sintering temperature is 600-900°C.
[0049] The seed crystals are produced through a pressurized sintering process, performed at a higher temperature than that of standard materials and with a longer hold time to promote grain growth. Ceramic sintering theory indicates that each grain is a single crystal with minimal lattice defects. No inorganic or organic carbon sources are added during the seed crystal preparation process, and grain growth is limited only by the kinetics of sintering temperature and time, not by the physical constraints of carbon coating. Therefore, the grains grow very easily, with a primary particle size of 200-800 microns. The seed crystal particle size is controlled by pulverization to a range of 0.01-2 μm. Only by keeping the seed crystals within a small particle size range can the particle size of the polyanion powder material induced by the seed crystals be guaranteed to be 5-20 μm.
[0050] In some preferred embodiments, in step S2, the spray drying process is as follows:
[0051] The inlet air temperature range is 180-240℃, the outlet air temperature range is 90-120℃, and the centrifugal speed range is 25000-35000r / min.
[0052] In some preferred embodiments, in step S3, the step-by-step sintering includes a first sintering step and a second sintering step; the first sintering step has a heating rate of 1-10°C / min, a sintering temperature of 300-400°C, and a holding time of 1-5h;
[0053] The second sintering process is as follows: the sintering temperature is 450-800° C., and the holding time is 2-5 hours.
[0054] In some preferred embodiments, in step S3, the flow rate of the inert gas is 10-300 ml / min; and the purity of the inert gas is not less than 99.99%.
[0055] An embodiment of the present invention further provides a composite polyanion powder material, which is prepared by the above-mentioned preparation method; the composite polyanion powder material includes a polyanion material and a carbon material.
[0056] In addition, an embodiment of the present invention further provides a battery electrode, comprising the above-mentioned composite polyanion powder material.
[0057] In addition, an embodiment of the present invention further provides a sodium ion battery, comprising the above-mentioned battery electrode.
[0058] The present invention will be further described below with reference to the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. However, the embodiments are not intended to limit the present invention.
[0059] The preparation method of the seed crystal used in the following examples is:
[0060] A precursor source, dispersant, and solvent are mixed in a specific ratio to form a seed crystal mixture. The solvent in the seed crystal mixture is removed by spray drying to obtain a seed crystal precursor intermediate. The seed crystal precursor intermediate is then subjected to static pressing to form a ceramic green body, which is then sintered at high temperature and crushed to obtain the seed crystal. The static pressing pressure is 150 MPa, and the high-temperature sintering temperature is 750°C. The crushed seed crystal has a particle size of 0.05 μm.
[0061] Example 1
[0062] This embodiment relates to a method for preparing a composite polyanion powder material, which specifically includes the following steps:
[0063] S1. Preparation of mixed slurry of precursors: The precursor sources ammonium dihydrogen phosphate, ferrous oxalate, and sodium carbonate are dissolved in 10L deionized water in a molar ratio of 4:1.5:2 (calculated based on a total mass of 1kg), and 20g of polyacrylic acid is added at 2wt% of the total solid mass, and mixed and stirred. The entire slurry preparation process uses a 20L wet vertical external circulation ball mill, and the stirring speed is set to 30Hz for ball milling for 1 hour to obtain mixed slurry 1; 10wt% of the total solid mass of carbon source (50g acetylene black and 50g glucose) is added to the mixed slurry 1 and mixed and ball milled for 2h, and then 50g Na4Fe3(PO4)2P2O7 (abbreviated as NFPP) is added again as a seed crystal and added to the mixed slurry 1 to obtain mixed slurry 2 for standby use.
[0064] S2. Preparation of precursor mixed powder: The mixed slurry 2 obtained in step S1 is spray-dried to remove the solvent, and the peristaltic pump feed rate is set to 120 ml / min, the atomizing disk speed is set to 30,000 r / min, the inlet air temperature is set to 230°C, and the outlet air temperature is set to 105°C; the spray-dried precursor mixed powder is obtained for standby use.
[0065] S3. Sintering synthesis of polyanion materials: The precursor powder obtained in step S2 is filled into a graphite crucible, and 99.99% nitrogen is introduced as a protective atmosphere. The heating rate is set to 5°C / min to 350°C and kept warm for 2 hours to crack the organic-coated carbon and remove the crystallization water of the precursor and the solid-phase reaction tail gas. The temperature is continued to be raised to 550°C at 3°C / min and kept warm for 3 hours. After air flow pulverization, demagnetization is performed to obtain a composite polyanion powder material.
[0066] Example 2
[0067] This embodiment relates to a method for preparing a composite polyanion powder material, which specifically includes the following steps:
[0068] S1. Preparation of mixed slurry of precursors: Dissolve the precursor sources ammonium dihydrogen phosphate, titanium dioxide, and sodium carbonate in 10L deionized water at a molar ratio of 3:1:0.5 (calculated based on a total mass of 1kg), and add 20g of polyacrylic acid at 2wt% of the total solid mass, and mix and stir. The entire slurry preparation process uses a 20L wet vertical external circulation ball mill, set the stirring speed to 30Hz, and ball mill for 1 hour to obtain mixed slurry 1; add 10wt% of the total solid mass of carbon source (50g acetylene black and 50g glucose) to the mixed slurry 1, mix and ball mill for 2h, and then add 50g NaTi2(PO4)3 (abbreviated as NTP) powder again as a seed crystal and ball mill for 2 hours to obtain mixed slurry 2 for standby use.
[0069] S2. Preparation of precursor mixed powder: The mixed slurry 2 obtained in step S1 is spray-dried to remove the solvent, and the peristaltic pump feed rate is set to 120 ml / min, the atomizing disk speed is set to 30,000 r / min, the inlet air temperature is set to 230°C, and the outlet air temperature is set to 105°C; the spray-dried precursor mixed powder is obtained for standby use.
[0070] S3. Sintering synthesis of polyanion materials: The precursor powder obtained in step S2 is filled into a graphite crucible, and 99.99% nitrogen is introduced as a protective atmosphere. The heating rate is set to 5°C / min to 350°C and kept warm for 2 hours to crack the organic-coated carbon and remove the crystallization water of the precursor and the solid-phase reaction tail gas. The temperature is continued to be raised to 750°C at 4°C / min and kept warm for 3 hours. After air flow pulverization, demagnetization is performed to obtain a composite polyanion powder material.
[0071] Comparative Example 1
[0072] This comparative example relates to a method for preparing a composite polyanion powder material. The only difference between this comparative example and Example 1 is that no seed crystals are added in step S1. The other operations are the same. The specific steps of S1 are as follows:
[0073] The precursor sources ammonium dihydrogen phosphate, ferrous oxalate, and sodium carbonate were dissolved in 10L of deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1kg), and 20g of polyacrylic acid was added at 2wt% of the total solid mass, and mixed and stirred. The entire slurry preparation process used a 20L wet vertical external circulation ball mill, set the stirring speed to 30Hz, and ball milled for 1 hour to obtain mixed slurry 1; 10wt% of the total solid mass of carbon source (50g acetylene black and 50g glucose) was added to the mixed slurry 1 and mixed and ball milled for 2h to obtain mixed slurry 2.
[0074] Comparative Example 2
[0075] This comparative example relates to a method for preparing a composite polyanion powder material. The only difference between this comparative example and Example 2 is that no seed crystals are added in step S1. The other operations are the same. The specific steps of S1 are as follows:
[0076] The precursor sources ammonium dihydrogen phosphate, titanium dioxide, and sodium carbonate were dissolved in 10L of deionized water at a molar ratio of 3:1:0.5 (calculated based on a total mass of 1kg), and 20g of polyacrylic acid was added at 2wt% of the total solid mass, and mixed and stirred. The entire slurry preparation process used a 20L wet vertical external circulation ball mill, set the stirring speed to 30Hz, and ball milled for 1 hour to obtain mixed slurry 1; 10wt% of the total solid mass of carbon source (50g acetylene black and 50g glucose) was added to the mixed slurry 1 and mixed and ball milled for 2h to obtain mixed slurry 2.
[0077] Comparative Example 3
[0078] This comparative example relates to a method for preparing a composite polyanion powder material. The only difference between this comparative example and Example 1 is that no carbon source is added in step S1, and the rest of the operations are the same. The specific steps of S1 are as follows:
[0079] The precursor sources ammonium dihydrogen phosphate, ferrous oxalate, and sodium carbonate were dissolved in 10L of deionized water at a molar ratio of 4:1.5:2 (calculated based on a total mass of 1kg), and 20g of polyacrylic acid was added at 2wt% of the total solid mass, and mixed and stirred. The entire slurry preparation process used a 20L wet vertical external circulation ball mill, set the stirring speed to 30Hz, and ball milled for 1 hour to obtain mixed slurry 1; 50gNa4Fe3(PO4)2P2O7 was added to the mixed slurry 1 as a seed crystal and added to the mixed slurry 1 to obtain mixed slurry 2.
[0080] Comparative Example 4
[0081] This comparative example relates to a method for preparing a composite polyanion powder material. The only difference between this comparative example and Example 2 is that no carbon source is added in step S1, and the rest of the operations are the same. The specific steps of S1 are as follows:
[0082] The precursor sources ammonium dihydrogen phosphate, titanium dioxide, and sodium carbonate were dissolved in 10L of deionized water at a molar ratio of 3:1:0.5 (calculated based on a total mass of 1kg), and 20g of polyacrylic acid was added at 2wt% of the total solid mass, and mixed and stirred. The entire slurry preparation process used a 20L wet vertical external circulation ball mill, set the stirring speed to 30Hz, and ball milled for 1 hour to obtain mixed slurry 1; 50g of NaTi2(PO4)3 powder was added to the mixed slurry 1 as a seed crystal and ball milled for 2 hours to obtain mixed slurry 2.
[0083] Comparative Example 5
[0084] This comparative example relates to a method for preparing a composite polyanion powder material. The only difference between this comparative example and Example 1 is that in Example 1, step S1 does not contain an inorganic carbon source. The specific operating steps are as follows:
[0085] Preparation of mixed slurry of precursor: The precursor sources ammonium dihydrogen phosphate, titanium dioxide, and sodium carbonate are dissolved in 10L deionized water in a molar ratio of 3:1:0.5 (calculated based on a total mass of 1kg), and 20g of polyacrylic acid is added at 2wt% of the total solid mass, and mixed and stirred. The entire slurry preparation process uses a 20L wet vertical external circulation ball mill, and the stirring speed is set to 30Hz for ball milling for 1 hour to obtain mixed slurry 1; 10wt% of the total solid mass of carbon source (100g glucose) is added to the mixed slurry 1 and mixed and ball milled for 2h, and then 50g NaTi2(PO4)3 (abbreviated as NTP) powder is added again as a seed crystal and ball milled for 2 hours to obtain mixed slurry 2 for standby use.
[0086] Characterization and performance testing
[0087] 1. Characterization of the composite polyanion powder materials prepared in the above examples and comparative examples
[0088] Figure 1This is a schematic diagram of seed-induced crystal growth. The presence of seed crystals provides multi-site crystal growth, making it easier to overcome the crystal formation energy barrier. This reduces the calcination temperature and holding time during the crystal formation stage, thereby reducing energy consumption. Furthermore, because the seed crystals are obtained by crushing large single crystals, they have a high degree of crystallization and few lattice defects, significantly improving the purity and crystallinity of the resulting powder. This makes it particularly suitable for the large-scale preparation of polyanionic powder materials and the synthesis of high-purity, low-defect crystals. Image analysis software was used to automatically measure the diameter of each grain in the composite polyanionic powder materials prepared in the Examples and Comparative Examples. 300 grains were measured to obtain the average grain size and variance. The results are shown in Table 1.
[0089] Table 1
[0090] Serial number Average grain size (μm) <![CDATA[Grain size variance (μm 2 )]]> Example 1 6.7 1.5 Example 2 17.6 3.2 Comparative Example 1 3.5 34.1 Comparative Example 2 14.5 21.2 Comparative Example 3 54.7 11.5 Comparative Example 4 94.8 18.9 Comparative Example 5 35.4 7.5
[0091] As shown in Table 1, compared to Comparative Examples 1 and 2, the data from Examples 1 and 2 show that the polyanion powder materials with seed crystal induction have more uniform morphology and larger crystal size. However, the grains with grain induction but without organic or inorganic carbon coating exhibit abnormal grain growth (Comparative Examples 3 and 4). This is because the inorganic and organic carbon sources are evenly coated on the surface of the seed crystals and powder, acting as a "pinning" force and suppressing abnormal grain growth. In Comparative Example 5, only organic carbon was used to coat the polyanion powder, resulting in larger polyanion powders. This is attributed to the absence of inorganic carbon, which cannot act as a powder barrier.
[0092] like Figure 2 and 3 The following are scanning electron micrographs of the composite polyanion powder materials prepared in Example 2 and Comparative Example 2. The results show that the polyanion material with seed crystal induction has a more uniform morphology and larger crystal size. The crystal diffraction peaks tested by XRD are more obvious, and no impurity phase is generated. In contrast, the polyanion material without seed crystal induction has no obvious diffraction peaks, has impurity peaks, and the purity of the synthesized crystals is poor ( Figure 4 and Figure 5 ).
[0093] 2. Application
[0094] Preparation of positive electrode: The prepared composite polyanion powder material, superP, and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1, and NMP was added and stirred to obtain a positive electrode active slurry. The positive electrode active slurry was evenly coated on the surface of the aluminum foil current collector, and a 200 μm doctor blade was used to prepare the electrode. After drying at 100°C for 10 hours, the electrode film was punched into an electrode with a diameter of 14 mm. The surface density of the active material was 2.5 mg cm -2 .
[0095] Battery Assembly: The positive electrode, electrolyte, Celgard polypropylene film, and sodium metal negative electrode were assembled to form a button half-cell. The electrolyte was 1 mol / L NaPF6, and the electrolyte solvent was a mixed solvent with a volume ratio of EC:DMC:EMC = 1:1:1.
[0096] Test conditions: The test was conducted in the voltage range of 1.2-4.2V, the specific capacity of the battery was tested at 0.1C, and the cycle performance of the battery was tested at a charge and discharge rate of 1C. The capacity decay rate per 100 cycles was calculated as R = 100 * (initial specific capacity - specific capacity after cycle) / (initial specific capacity * number of cycles) * 100%.
[0097] Table 2
[0098]
[0099]
[0100] As shown in Table 2, the specific capacity of the battery prepared in Example 1 at 0.1C is much greater than that of the battery assembled with the powder material of the comparative example. This is because the composite polyanion powder material prepared in the comparative example has abnormally grown grains, which greatly increases the diffusion impedance of ions and thus reduces the specific capacity of the material. The composite polyanion powder materials synthesized with seed crystal induction in Example 1 and Example 2 show better cycle performance ( Figure 6 and Figure 7 ), while the specific capacity performance of Comparative Examples 3 and 4 is too low to be used for large-scale applications. This is because the seed crystal is a single crystal particle, and the single crystal has a regular and orderly atomic arrangement. When it is used as a "seed", the interface energy consumption of the raw materials reacting on its surface is low, and there are few defects (vacancies or impurities) inducing the formation of a complete three-dimensional periodic lattice structure; due to the few defects in the lattice, the deintercalation of ions during the electrochemical reaction will not affect the lattice structure, which in turn leads to good stability of the lattice (Example 1 and Example 2). The material synthesized without seed crystal induction may cause defects in the target synthetic material due to the presence of impurities, and the uneven grain size leads to different charge and discharge depths of different particles, causing the material cycle performance to deteriorate (Comparative Example 1 and Comparative Example 2). The powder material prepared in Comparative Example 5 without the addition of inorganic carbon to the mixture exhibits a lower capacity, which is mainly due to the abnormal growth of the seed crystal.
[0101] The above embodiments are merely preferred embodiments for the purpose of fully illustrating the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are within the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
Claims
1. A method for preparing a composite polyanion powder material, characterized in that: The following steps are involved: S1, mixing a precursor source, a dispersant, an organic carbon source, an inorganic carbon source, a seed crystal and a solvent to form a precursor mixture; the precursor source includes a sodium source, a transition metal source and an anion source; the seed crystal has the same crystal form as the polyanion material in the composite polyanion powder material; the mass ratio of the organic carbon source and the inorganic carbon source to the precursor source is 5-10wt%; S2, removing the solvent in the precursor mixture described in S1 by spray drying technology to obtain a precursor intermediate; S3, sintering, airflow crushing and demagnetizing the precursor intermediate in step S2 in an inert gas environment to obtain the composite polyanion powder material.
2. The preparation method according to claim 1, characterized in that In step S1, the mass ratio of the seed crystal to the precursor source in the precursor mixture is 1-5:
100.
3. The preparation method according to claim 1, characterized in that: In step S1, the seed crystal has a particle size of 0.01-2 um; the seed crystal is prepared by pressure sintering, and the preparation method is as follows: A precursor source, a dispersant and a solvent are mixed to form a seed crystal mixture; the solvent in the seed crystal mixture is removed by spray drying technology to obtain a seed crystal precursor intermediate; the seed crystal precursor intermediate is statically pressed to prepare a ceramic blank, and the seed crystal is obtained after high-temperature sintering and crushing.
4. The preparation method according to claim 1, characterized in that: In step S1, the inorganic carbon source is selected from one or more of acetylene black, Ketjen black, graphite, activated carbon and carbon nanospheres; The organic carbon source is selected from one or more of glucose, sucrose, starch, polyethylene glycol, polyvinyl alcohol, polyacrylic acid and citric acid.
5. The preparation method according to claim 1, characterized in that: In step S1, the mixing is ball milling mixing, the rotation speed of the ball mill is 100-500r / min, the ball milling beads are made of zirconium oxide, the diameter of the ball milling beads is 3-10mm, and the ball milling time is 2-6h; the solid content of the mixture is 20-60wt%.
6. The preparation method according to claim 1, characterized in that: In step S2: In the spray drying step: the air inlet temperature ranges from 180 to 240° C., the air outlet temperature ranges from 90 to 120° C., and the centrifugal speed ranges from 25,000 to 35,000 r / min.
7. The preparation method according to claim 1, characterized in that: In step S3: The sintering includes a first step of sintering and a second step of sintering; in the first step of sintering, the heating rate is 1-10°C / min, the sintering temperature is 300-400°C, and the holding time is 1-5h; In the second step of sintering treatment, the sintering temperature is 450-800°C and the holding time is 2-5h; The flow rate of the inert gas is 10-300 ml / min; the purity of the inert gas is not less than 99.99%.
8. A composite polyanion powder material, characterized in that: Prepared by the preparation method described in any one of claims 1-7; the composite polyanion powder material comprises a polyanion material and a carbon material.
9. A battery pole piece, characterized in that: Including the composite polyanion powder material as described in claim 8.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the battery pole piece according to claim 9.
Citation Information
Patent Citations
Preparation method of single-crystal nickel cobalt lithium manganate ternary material
CN113299905A
Composite carbon source coated composite sodium ferric phosphate positive electrode material and preparation method thereof
CN116885150A
Cited By
Polyanionic sodium-ion battery positive electrode material as well as preparation method and application thereof
CN122619794A