Nanometer strip-shaped aluminum oxide as well as preparation method and application thereof
By controlling the pH value and hydrothermal reaction, nano-strip-shaped alumina was prepared, which solved the problems of non-concentrated particle size distribution and irregular shape of alumina in the existing technology, and improved thermal conductivity and insulation properties, making it suitable for thermally conductive inks.
Patent Information
- Application Number
- CN202411007703.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing alumina preparation technology is complex, and the particle size distribution of nano-alumina is not concentrated and the shape is irregular, resulting in insufficient thermal conductivity and affecting the quality of thermally conductive electronic inks.
Nano-sized alumina strips were prepared by mixing an aqueous solution of aluminum sulfate octadeca and sodium hydroxide, controlling the pH value to 4-5, carrying out a high-temperature hydrothermal reaction, and then calcining it under atmospheric conditions to ensure a concentrated particle size distribution.
High-purity, concentrated particle size, and uniform shape nano-strip alumina were prepared, which improves thermal conductivity and insulation properties, making it suitable for thermally conductive inks and enhancing the heat dissipation effect of electronic devices.
Smart Images

Figure CN118908253A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to nano strip aluminum oxide and a preparation method and application thereof. Background Art
[0002] The main function of thermal conductive electronic ink is to give products excellent heat dissipation function, and it has broad application prospects in the field of microelectronics. As an important branch of functional ink, thermal conductive electronic ink not only has packaging and decoration functions, but also significantly improves the heat dissipation function of products through its special composition and preparation method.
[0003] The role of nano-alumina in thermal conductive electronic ink is to improve the insulation and thermal conductivity of the ink. As a multifunctional nanomaterial, nano-alumina has demonstrated its unique properties and application potential in many fields. In thermal conductive electronic ink, the addition of nano-alumina significantly improves the insulation and thermal conductivity of the ink. Specifically, the addition of nano-alumina can form a thermal conductive network chain, thereby significantly improving the thermal conductivity of the ink. At the same time, since nano-alumina has excellent electrical insulation and stability, its addition can also significantly improve the insulation performance of the ink, ensuring the safe and stable operation of electronic equipment.
[0004] In the existing alumina preparation technology, the preparation process is complicated, the particle size distribution of the obtained nano alumina is not concentrated, and the shape of the nano alumina is irregular or mostly granular. When it is used to prepare thermally conductive electronic ink, the thermal conductivity is insufficient, making the quality of the electronic ink not outstanding enough. Summary of the invention
[0005] In view of this, the main technical problem solved by the present invention is to prepare a nano-strip aluminum oxide with better thermal conductivity, high purity and concentrated particle size distribution.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0007] A method for preparing nano-strip aluminum oxide comprises the following steps:
[0008] An aqueous solution of aluminum sulfate 18hydrate and an aqueous solution of sodium hydroxide are mixed and reacted to generate aluminum hydroxide;
[0009] placing the mixed solution into a hydrothermal reactor for high-temperature hydrothermal reaction;
[0010] The nano-strip aluminum oxide is obtained by calcining at 1000-1200° C. in an atmospheric atmosphere.
[0011] In the present invention, the molar ratio of aluminum sulfate 18hydrate to sodium hydroxide in the aqueous solution of aluminum sulfate 18hydrate and the aqueous solution of sodium hydroxide is 1:3.
[0012] During the mixing process of the two solutions, the pH value of the solution must always be maintained at 4-5. Since the aqueous solution of aluminum sulfate 18hydrate is acidic, the amount of the aqueous solution of aluminum sulfate 18hydrate added during the mixing process is kept greater than the amount of the aqueous solution of sodium hydroxide added, thereby controlling the pH value during the mixing process to be lower.
[0013] In the present invention, an aqueous solution of aluminum sulfate 18hydrate and an aqueous solution of sodium hydroxide are mixed to generate aluminum hydroxide precipitate. During the solution mixing process, the generated aluminum hydroxide is greatly affected by the pH value of the solution. Maintaining the solution to be acidic can ensure the smooth generation of aluminum hydroxide.
[0014] After the addition of the aqueous solution of aluminum sulfate 18hydrate is completed, the remaining aqueous solution of sodium hydroxide is continued to be added, and then the pH of the mixed solution is adjusted to 5.5-7.5. Within this pH value range, the aluminum hydroxide precipitate in the solution is in a very sensitive state, so that in further hydrothermal treatment, the sensitive aluminum hydroxide is recrystallized from dispersed fine grains under hydrothermal conditions, and the aluminum hydroxide crystals grow axially. Finally, during calcination, based on the shape of the aluminum hydroxide crystals, a nano-alumina product in the form of long strips is obtained, and the particle size distribution of the nano-alumina is relatively concentrated.
[0015] As a preferred embodiment of the present invention, the substance added to adjust the pH value of the mixed solution in the present invention is preferably ammonia water, which has the advantage of not introducing other impurities after addition. In addition, in the subsequent hydrothermal step, ammonia water will have gas overflow at high temperature, increasing the pressure in the hydrothermal reactor, and the hydrothermal efficiency is higher.
[0016] As a preferred embodiment of the present invention, the mass percentage concentration of the ammonia water is 20-23wt%.
[0017] As a preferred embodiment of the present invention, the concentration of the aqueous solution of aluminum sulfate 18hydrate is 100g / mL, and the concentration of the aqueous solution of sodium hydroxide is 18g / mL; the volume ratio of the aqueous solution of aluminum sulfate 18hydrate to the aqueous solution of sodium hydroxide is 1:1, and the mixing process of the aqueous solution of aluminum sulfate 18hydrate and the aqueous solution of sodium hydroxide is mixed by dropping under stirring, and the dropping method is adopted to directly generate aluminum hydroxide precipitation. The dropping speed is preferably 20-50ml / min, and the dropping speed of the aqueous solution of aluminum sulfate 18hydrate is greater than the dropping speed of the aqueous solution of sodium hydroxide to ensure that the pH in the mixed solution is 4-5.
[0018] As a preferred embodiment of the present invention, the hydrothermal reaction kettle is at a temperature of 120 to 140° C., and the hydrothermal reaction time is 2 to 4 hours.
[0019] As a preferred embodiment of the present invention, the calcination time of aluminum hydroxide is 1 to 3 hours.
[0020] As a preferred embodiment of the present invention, the aluminum hydroxide is filtered and washed with water before calcination, and then dried.
[0021] The nano-aluminum oxide prepared by the present invention is in the form of long strips, with uniform shape and high purity. The particle size is mainly concentrated in the range of 50.75nm to 91.28nm, and it has a larger specific surface area. It is used as a thermally conductive filler in the preparation of thermally conductive ink. The long strip structural feature can play a better connecting role, and the thermal conduction path is shorter, so it can be expected that the product has a better thermal conductivity effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is one of the SEM images of the long strip of aluminum oxide of the preferred embodiment of the present invention;
[0023] Figure 2 The second SEM image of the long strip of aluminum oxide of the preferred embodiment of the present invention;
[0024] Figure 3 This is a Malvern particle size distribution instrument test result diagram of the long strip of aluminum oxide in the preferred embodiment of the present invention;
[0025] Figure 4 is a SEM image of the aluminum oxide of Comparative Example 1 of the present invention;
[0026] Figure 5 This is a SEM image of the aluminum oxide of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0027] In order to allow those skilled in the art to understand the present invention more clearly and intuitively, the present invention will be further described below in conjunction with the accompanying drawings.
[0028] The method for preparing nano-strip aluminum oxide of the present invention comprises the following steps:
[0029] Mixing an aqueous solution of aluminum sulfate 18hydrate and an aqueous solution of sodium hydroxide, wherein the pH of the solution during the mixing process is 4 to 5;
[0030] The mixed solution is placed in a hydrothermal reactor for high-temperature hydrothermal reaction; the condition of the hydrothermal reactor is 120-140° C., and the hydrothermal reaction time is 2-4 hours; the aluminum hydroxide is filtered and washed with water, and then dried;
[0031] The nano-strip aluminum oxide is obtained by calcining at 1000-1200° C. for 1-3 hours in an atmospheric atmosphere.
[0032] After the mixing of the aqueous solution of aluminum sulfate 18hydrate and the aqueous solution of sodium hydroxide is complete, the pH of the mixed solution is adjusted to 5.5 to 7.5.
[0033] The substance added to adjust the pH value of the mixed solution in the present invention is preferably ammonia water, which has the advantage of not introducing other impurities after addition. In addition, in the subsequent hydrothermal step, ammonia water will have gas overflow at high temperature, increasing the pressure in the hydrothermal reactor, and the hydrothermal efficiency is higher.
[0034] The mass percentage concentration of the ammonia water is 20-23wt%.
[0035] The volume ratio of the aqueous solution of aluminum sulfate 18hydrate to the aqueous solution of sodium hydroxide is 1:1. The aqueous solution of aluminum sulfate 18hydrate and the aqueous solution of sodium hydroxide are mixed by dropwise addition, and the dropwise addition speed is preferably 20-50 ml / min.
[0036] Preferred Embodiments
[0037] The method for preparing aluminum oxide in this embodiment comprises the following steps:
[0038] Add deionized water to aluminum sulfate 18hydrate in a beaker to dissolve it into an aqueous solution with a concentration of 100 g / L, and add deionized water to sodium hydroxide in a beaker to dissolve it into an aqueous solution with a concentration of 18 g / L;
[0039] Add 100 ml of bottom water to a 2000 ml beaker; in the embodiment, a stirring blade is provided in the reactor, and the addition of bottom water can ensure that the aluminum sulfate 18hydrate and sodium hydroxide added dropwise can react quickly during stirring during the initial reaction;
[0040] Take 500ml of aluminum sulfate 18hydrate aqueous solution and 500ml of sodium hydroxide aqueous solution respectively, start stirring, add the aluminum sulfate 18hydrate aqueous solution and the sodium hydroxide aqueous solution to the beaker by dropwise addition, in this process, ensure that the amount of aluminum sulfate 18hydrate aqueous solution added is greater than the amount of sodium hydroxide aqueous solution added, and the excessive addition of aluminum sulfate 18hydrate can control the pH value of the solution to be maintained at 4-5, and a white aluminum hydroxide precipitate will be generated during the dropwise mixing process. The reaction in the beaker is uniform and stable during the dropwise addition process. Compared with the large reaction fluctuation when the two are directly poured together, the uniformity of the synthetic particle size is poor. The aluminum hydroxide particle size generated by the slow dropwise addition is better controlled, uniform and has good particle size concentration. The dripping speed of the aluminum sulfate 18hydrate aqueous solution and the sodium hydroxide aqueous solution is 20-50ml / min. By controlling the dripping speed of the aluminum sulfate 18hydrate aqueous solution to be greater than the dripping speed of the aluminum hydroxide aqueous solution, the pH of the mixed solution can be controlled to 4.0-5.0 with a pH meter, and after the two solutions are added, 20-23wt% of ammonia water is added to adjust the pH to 5.5-7.5. The mixed solution was then placed in a hydrothermal reactor, hydroheated at 120°C for 4 hours, taken out, filtered and washed, and the filter cake obtained was dried at 105°C. The dried sample was placed in a calcining furnace and calcined at 1100°C for 2 hours in an atmospheric atmosphere to obtain strip-shaped alumina.
[0041] In this embodiment, the aluminum sulfate 18hydrate raw material is purified before use to remove trace amounts of heavy metal impurities.
[0042] The test standard of the alumina product in this embodiment is: GB / T 24487-2022;
[0043] The alumina particle size was tested by Malvern particle size distribution instrument;
[0044] The whiteness of alumina is tested by Minolta Whiteness Tester 2600d;
[0045] Alumina metal is tested by Shimadzu atomic absorption furnace.
[0046] The purity of the prepared aluminum oxide was tested, and the purity of the aluminum oxide reached 99.78%. The test results are shown in Table 1.
[0047] Table 1
[0048]
[0049] In addition, the aluminum oxide was scanned by electron microscope, and the results were as follows Figure 1-2 As shown, the particle size of the aluminum oxide prepared in this example is close to the result of the particle size distribution instrument test.
[0050] In this embodiment, the aluminum hydroxide generated by the mixed solution undergoes hydrothermal treatment. During this process, the aluminum hydroxide is regrown under the conditions of high-temperature hydrothermal reaction to remove the ions adsorbed on the surface. At the same time, the aluminum hydroxide grows axially during the re-growth process, and the crystals grow again into strip-shaped aluminum oxide with uniform particle size and shape. The morphology and particle size of the aluminum oxide obtained by calcining the aluminum hydroxide are also directly affected, and the quality is improved. The aluminum oxide product obtained by calcining is tested by a Malvern particle size distribution instrument, and it is found that the particle size of the aluminum oxide is mainly concentrated in the range of 50.75nm to 91.28nm (the results are shown in FIG. Figure 3 shown).
[0051] Comparative Example 1
[0052] The difference between this embodiment and the preferred embodiment is that no hydrothermal treatment is performed. The specific preparation process is as follows:
[0053] Add deionized water to aluminum sulfate 18hydrate in a beaker to dissolve it into an aqueous solution with a concentration of 100 g / L. Add deionized water to sodium hydroxide in a small cup to dissolve it into an aqueous solution with a concentration of 18 g / L.
[0054] Add 100 ml of bottom water to a 2000 ml beaker; the reactor is equipped with a stirring blade, and the addition of bottom water can ensure that the aluminum sulfate 18hydrate and sodium hydroxide added dropwise can fully react during the stirring during the initial reaction;
[0055] Take 500ml of aluminum sulfate 18hydrate aqueous solution and 500ml of sodium hydroxide aqueous solution respectively, start stirring, add the aluminum sulfate 18hydrate aqueous solution and the sodium hydroxide aqueous solution to the beaker by dropwise addition, in this process, ensure that the amount of aluminum sulfate 18hydrate aqueous solution added is greater than the amount of sodium hydroxide aqueous solution added, and the excessive addition of aluminum sulfate 18hydrate can control the pH value of the solution to be maintained at 4-5, and a white aluminum hydroxide precipitate will be generated during the dropwise mixing process. The dripping speed of the aluminum sulfate 18hydrate aqueous solution and the sodium hydroxide aqueous solution is 20-50ml / min, and the pH of the mixed solution can be controlled to be 4.0-5.0 by controlling the dripping speed of the aluminum sulfate 18hydrate aqueous solution to be greater than the dripping speed of the aluminum hydroxide aqueous solution, and the pH value meter can be used to control the pH of the mixed solution to be 4.0-5.0. After the two solutions are added, add 20-23wt% of ammonia water to adjust the pH to 5.5-7.5. The filter cake obtained after suction filtration and water washing is dried at 105°C, and the dried sample is directly placed in a calcining furnace and calcined at 1100°C for 2h in an atmospheric atmosphere.
[0056] Aluminum sulfate 18hydrate reacts with sodium hydroxide to generate aluminum hydroxide. The aluminum hydroxide has not been subjected to hydrothermal treatment, so the aluminum hydroxide is gradually generated during the dropwise addition process. Without hydrothermal reaction and recrystallization, the aluminum hydroxide aggregates into agglomerates, and the structural quality of the aluminum oxide obtained by calcination is affected. The aluminum oxide obtained in Comparative Example 1 was scanned by an electron microscope, and the results are as follows: Figure 4 As shown, it can be seen that the alumina prepared without hydrothermal reaction aggregates into agglomerates.
[0057] Comparative Example 2
[0058] The difference between this embodiment and the preferred embodiment is that the pH of the solution is not controlled. The specific preparation process is as follows:
[0059] Add deionized water to aluminum sulfate 18hydrate in a beaker to dissolve it into an aqueous solution with a concentration of 100 g / L, and add deionized water to sodium hydroxide in a beaker to dissolve it into an aqueous solution with a concentration of 18 g / L;
[0060] Add 100 ml of bottom water to a 2000 ml beaker; in the embodiment, a stirring blade is provided in the reactor, and the addition of bottom water can ensure that the aluminum sulfate 18hydrate and sodium hydroxide added dropwise can react quickly during stirring during the initial reaction;
[0061] Take 500ml of aluminum sulfate 18hydrate aqueous solution and 500ml of sodium hydroxide aqueous solution respectively, start stirring, and add the aluminum sulfate 18hydrate aqueous solution and sodium hydroxide aqueous solution to the beaker by dropwise addition. In this process, the aluminum sulfate 18hydrate aqueous solution and the sodium hydroxide aqueous solution are added in equal amounts, and a white aluminum hydroxide precipitate will be generated during the gradual dropwise mixing process. The dripping rate of the aluminum sulfate 18hydrate aqueous solution and the sodium hydroxide aqueous solution is 40ml / min. After the two solutions are added, the mixed solution is placed in a hydrothermal reactor, and is taken out after hydrothermal treatment at 120°C for 4h. The filter cake obtained after filtration and washing is dried at 105°C. The dried sample is placed in a calcining furnace and calcined at 1100°C for 2h in an atmospheric atmosphere to obtain strip-shaped aluminum oxide.
[0062] In this comparative example 2, aluminum sulfate 18hydrate and sodium hydroxide react to generate aluminum hydroxide. The pH value of the mixed solution is not controlled during the dropwise addition process and after the dropwise addition. Therefore, aluminum hydroxide is gradually generated during the dropwise addition process. Aluminum hydroxide can be recrystallized into granular form during the hydrothermal process, and the aluminum oxide obtained by calcination is also granular. The aluminum oxide obtained in comparative example 2 is scanned by an electron microscope, and the results are as follows: Figure 5 As shown, it can be seen that although recrystallization can be formed without agglomeration during hydrothermal treatment without adjusting the pH, and the particle size of aluminum oxide is relatively concentrated, aluminum hydroxide does not have the ability to grow axially during the hydrothermal reaction, and the shape of aluminum oxide does not have a specific strip structure.
[0063] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing nano-strip aluminum oxide, characterized in that: The steps include: An aqueous solution of aluminum sulfate 18hydrate and an aqueous solution of sodium hydroxide are mixed and reacted to generate aluminum hydroxide; placing the mixed solution into a hydrothermal reactor for high-temperature hydrothermal reaction; The nano-strip aluminum oxide is obtained by calcining at 1000-1200°C in an atmospheric atmosphere; During the mixing process of the aqueous solution of aluminum sulfate 18hydrate and the aqueous solution of sodium hydroxide, the amount of the aqueous solution of aluminum sulfate 18hydrate added is kept greater than the amount of the aqueous solution of sodium hydroxide added so that the pH value of the solution is 4-5.
2. The method for preparing nano-strip aluminum oxide according to claim 1, characterized in that: After the solutions are mixed and reacted completely, the pH of the mixed solution is adjusted to 5.5-7.
5.
3. The method for preparing nano-strip aluminum oxide according to claim 2, characterized in that: The substance added to adjust the pH value of the mixed solution is ammonia water.
4. The method for preparing nano-strip aluminum oxide according to claim 3, characterized in that: The mass percentage concentration of the ammonia water is 20-23wt%.
5. The method for preparing nano-strip aluminum oxide according to claim 1, characterized in that: The concentration of the aqueous solution of aluminum sulfate 18hydrate is 100 g / mL, and the concentration of the aqueous solution of sodium hydroxide is 18 g / mL; The volume ratio of the aqueous solution of aluminum sulfate 18hydrate to the aqueous solution of sodium hydroxide is 1:1; The aqueous solution of aluminum sulfate 18hydrate and the aqueous solution of sodium hydroxide are mixed by dropwise addition, and the dropwise addition speed is preferably 20-50 ml / min.
6. The method for preparing nano-strip aluminum oxide according to claim 1, characterized in that: The hydrothermal reaction kettle temperature is 120-140°C, and the hydrothermal reaction time is 2-4 hours.
7. The method for preparing nano-strip aluminum oxide according to claim 1, characterized in that: The calcination time of aluminum hydroxide is 1 to 3 hours.
8. The method for preparing nano-strip aluminum oxide according to claim 1, characterized in that: Aluminum hydroxide is filtered and washed with water before calcination, and then dried.
9. Strip-shaped aluminum oxide obtained according to the preparation method according to any one of claims 1 to 8.
10. Use of the strip-shaped aluminum oxide prepared by the preparation method according to any one of claims 1 to 8 as a thermally conductive filler in the preparation of thermally conductive ink.
Citation Information
Patent Citations
Preparation method of flaky nano gamma-aluminum oxide
CN106276994A
Gamma-phase alumina nanotube and preparation method thereof
CN107500323A
Nanometer aluminium oxide and preparation method thereof
CN107879368A
Length-to-diameter-ratio-controllable AlOOH nano-adjuvant and preparation method thereof
CN109432417A