Gadolinium oxide doped cerium oxide nano composite material, preparation method thereof and solid oxide fuel cell
Through the complexation reaction of dextran with gadolinium and cerium and secondary calcination treatment, high-purity, low-cost gadolinium-doped cerium oxide nanocomposites are prepared, which solves the low life of yttrium oxide ceramic materials in solid oxide fuel cells. and the problem of not being suitable for large-scale production has achieved high efficiency, environmentally friendly preparation and electrochemical performance improvement of materials.
Patent Information
- Application Number
- CN202410963777.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The high working temperature of yttrium-stable zirconia ceramic materials in existing solid oxide fuel cells leads to low life and high production costs. The existing preparation methods are not environmentally friendly, have strong repeatability, and are not suitable for large-scale production.
Dextran is used as a macromolecular biological template to complex the mixed salt solution of gadolinium and cerium, and the gadolinium doped cerium oxide nanocomposite is prepared after secondary calcination to obtain high purity, low cost, suitable for large-scale production. Material.
The high purity and small particle size of the gadolinium-doped ceria nanocomposite are achieved, which simplifies the preparation process, reduces production costs, is suitable for industrial production, and improves electrochemical performance.
Smart Images

Figure CN118908265A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cell materials, and in particular relates to a gadolinium oxide-doped cerium oxide nanocomposite material and a preparation method thereof, and a solid oxide fuel cell. Background Art
[0002] With the continuous development of science and technology, people have gradually realized the impact of fossil fuels on the environment, including climate change, air pollution and resource depletion. Therefore, many scholars and researchers are exploring and developing various efficient and clean power generation technologies to reduce dependence on fossil fuels and promote sustainable development. Among them, fuel cells, as a power generation device that can directly convert chemical energy into electrical energy, generate electricity through electrochemical reactions, which usually involve the reaction of hydrogen as fuel (anode) and oxygen (cathode). Therefore, fuel cells have good environmental friendliness and high power generation efficiency in terms of clean and efficient power generation.
[0003] At present, the types of fuel cells mainly include proton exchange membrane fuel cells (PEMFC), solid oxide fuel cells (SOFC), molten carbonate fuel cells (MCFC) and phosphoric acid fuel cells (PAFC), etc. Among them, solid oxide fuel cells (SOFC) have been widely used in fixed or distributed power generation, vehicle auxiliary power supply and portable power supply due to their many advantages such as high energy conversion efficiency, strong fuel adaptability, all-solid-state structure, high power density, low greenhouse gas emissions, low noise and low environmental impact.
[0004] However, the solid oxide fuel cells disclosed in the prior art still have some problems during use, such as the high operating temperature (800-1000°C) of yttria-stabilized zirconia ceramic material (YSZ), which leads to a shorter life of the solid oxide fuel cell, increased production costs, and easy to cause side reactions between fuel cell components. In addition, the preparation methods of solid electrolytes generally include sol-gel method, coprecipitation method, ball milling method, calcination method or hydrothermal method, but the above methods have problems such as being environmentally unfriendly, complicated preparation process, non-repeatability, unsuitability for large-scale production, and high requirements for production equipment.
[0005] Therefore, in this field, there is an urgent need to develop a solid electrolyte material with high purity and good performance, and the corresponding preparation method is simple, efficient and suitable for large-scale production. Summary of the invention
[0006] In view of the shortcomings of the prior art, the object of the present invention is to provide a gadolinium oxide doped cerium oxide nanocomposite material and a preparation method thereof and a solid oxide fuel cell. The present invention provides a gadolinium oxide doped cerium oxide nanocomposite material with high purity, high specific surface area and small particle size, and the preparation method is simple and highly repeatable, which is conducive to large-scale industrial production.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a gadolinium oxide-doped cerium oxide nanocomposite material, the method comprising the following steps:
[0009] A mixed salt solution containing a gadolinium source and a cerium source is subjected to a complexation reaction with a dextran chelating agent to obtain a precursor material; the precursor material is subjected to a secondary calcination treatment to obtain a gadolinium oxide-doped cerium oxide nanocomposite material.
[0010] The present invention uses dextran as a macromolecular biotemplate, which loses protons in the solution and provides negatively charged binding sites, thereby being able to chelate metal cations. Compared with small molecule chelators, the long-chain macromolecular biotemplate provided by the present invention can maintain a good dispersion effect on metal cations, avoiding agglomeration between subsequently formed nanoparticles, and at the same time, the long-chain macromolecular biotemplate can help guide and regulate crystal growth, and finally obtain a powder with a small particle size and a high specific surface area. In addition, the present invention removes the dextran chelator through a secondary calcination process to obtain a high-purity gadolinium oxide-doped cerium oxide nanocomposite powder material.
[0011] The preparation method provided by the present invention has the advantages of simple operation, low cost, environmental friendliness and short preparation time, and the preparation method has high repeatability and is suitable for industrial production.
[0012] Preferably, the gadolinium source includes any one of hydrated gadolinium nitrate, hydrated gadolinium acetate or gadolinium acetylacetonate, or a combination of at least two thereof, preferably hydrated gadolinium acetate.
[0013] Preferably, the cerium source includes any one of hydrated cerium nitrate, hydrated cerium acetate, hydrated cerium carbonate, cerium ammonium nitrate or cerium acetylacetonate, or a combination of at least two thereof, preferably hydrated cerium acetate.
[0014] Preferably, the molar ratio of cerium ions in the cerium source to gadolinium ions in the gadolinium source is (2-15):1, preferably (4-9):1, for example, it can be 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, etc.
[0015] In the present invention, by adjusting the molar ratio of cerium ions in the cerium source to gadolinium ions in the gadolinium source, gadolinium oxide-doped cerium oxide nanocomposites with different preferred gadolinium doping amounts can be obtained, wherein when the molar ratio of cerium ions to gadolinium ions is 9:1 and 4:1, Ce, 0.9 G 0.1 0 1.95 (GDC10) and Ce 0.8 G 0.2 0 1.90 (GDC20). A molar ratio that is too high will result in insufficient gadolinium doping, thereby reducing the electrochemical performance of the gadolinium oxide-doped cerium oxide nanocomposite material. On the contrary, a molar ratio that is too high will result in greater lattice distortion and defects in the composite material, and reduce its overall performance.
[0016] Preferably, the total concentration of metal ions in the mixed salt solution is 0.05-5 mol / L, preferably 0.1-1 mol / L, for example, it can be 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, etc.
[0017] In the present invention, the mixed salt solution is obtained by mixing a solution containing a gadolinium source with a solution containing a cerium source, wherein the mixing is performed under stirring.
[0018] In the present invention, the stirring rate is 30-1000r / min, preferably 300-500r / min, for example, it can be 30r / min, 50r / min, 80r / min, 100r / min, 200r / min, 300r / min, 320r / min, 350r / min, 380r / min, 400r / min, 420r / min, 450r / min, 480r / min, 500r / min, 600r / min, 700r / min, 800r / min, 900r / min, 1000r / min and the like.
[0019] In the present invention, the stirring time is 0.5-24h, preferably 1.5h, for example, it can be 0.5h, 0.6h, 0.8h, 1h, 1.5h, 2h, 3h, 4h, 5h, 10h, 15h, 20h, 24h, etc.
[0020] Preferably, the mass ratio of the total mass of the gadolinium source and the cerium source to the dextran chelating agent is (0.1-100):1, preferably (1-20):1, for example, it can be 0.1:1, 0.5:1, 1:1, 2:1, 5:1, 6:1, 8:1, 10:1, 12:1, 15:1, 18:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 60:1, 70:1, 80:1, 90:1, 100:1, etc.
[0021] In the present invention, by adjusting the mass ratio of the total mass of the gadolinium source and the cerium source to the mass ratio of the dextran chelating agent, the dextran can play a good complexing role, thereby ensuring that the cerium ions and the gadolinium ions are uniformly precipitated and mixed. Too high a mass ratio will lead to uneven ion precipitation, and the metal cations cannot be dispersed in space, resulting in large-scale agglomeration. Otherwise, a large amount of carbon source impurities will be introduced, increasing the difficulty of obtaining pure powder by heat treatment.
[0022] Preferably, the complexing reaction is carried out under stirring.
[0023] Preferably, the stirring rate is 30-1000r / min, preferably 300-500r / min, for example, it can be 30r / min, 50r / min, 80r / min, 100r / min, 200r / min, 300r / min, 320r / min, 350r / min, 380r / min, 400r / min, 420r / min, 450r / min, 480r / min, 500r / min, 600r / min, 700r / min, 800r / min, 900r / min, 1000r / min and the like.
[0024] Preferably, the stirring time is 0.5-24 h, preferably 1.5 h, for example, it can be 0.5 h, 0.6 h, 0.8 h, 1 h, 2 h, 3 h, 4 h, 5 h, 10 h, 15 h, 20 h, 24 h, etc.
[0025] Preferably, the temperature of the complexing reaction is 60-100°C, preferably 70-90°C, for example, it can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.
[0026] In the present invention, the method of regulating the temperature of the complexing reaction exemplarily includes any one of water bath heating, oil bath heating, electric heating plate heating or flame heating, preferably water bath heating or electric heating plate heating.
[0027] Preferably, the complexing reaction further includes drying and grinding treatments in sequence.
[0028] Preferably, the drying temperature is 20-180°C, preferably 70-100°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 120°C, 150°C, 180°C, etc.
[0029] Preferably, the drying time is 2-72 h, preferably 6-14 h, for example, it can be 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, 14 h, 18 h, 20 h, 25 h, 30 h, 35 h, 40 h, 45 h, 50 h, 55 h, 60 h, 65 h, 70 h, 72 h, etc.
[0030] In the present invention, the grinding method includes manual grinding or ball milling, so as to break up the hard solid and provide more reaction contact sites, which is beneficial to remove residual organic matter such as dextran.
[0031] Preferably, the secondary calcination process includes a first calcination process and a second calcination process in sequence.
[0032] Preferably, the temperature of the first calcination treatment and the second calcination treatment are each independently 300-1200°C, preferably 600-900°C, for example, 300°C, 400°C, 500°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1100°C, 1200°C, etc.
[0033] Preferably, the heating rates of the first calcination treatment and the second calcination treatment are each independently 0.5-10°C / min, preferably 3-5°C / min, for example, 0.5°C / min, 1°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 6°C / min, 8°C / min, 10°C / min, etc.
[0034] Preferably, the time for the first calcination treatment and the second calcination treatment is independently 0.5-24h, preferably 2-6h, for example, it can be 0.5h, 0.6h, 0.8h, 1h, 2h, 3h, 4h, 5h, 6h, 8h, 10h, 15h, 20h, 24h, etc.
[0035] In the present invention, the first calcination treatment and the second calcination treatment both include grinding the calcined product after the calcination. Specifically, the grinding treatment after the first calcination treatment is to expose the carbon removal sites so as to better remove the carbon residues, thereby obtaining a high-purity gadolinium oxide-doped cerium oxide nanocomposite material. The grinding treatment after the second calcination treatment is to refine the powder particle size and make its particle size distribution more uniform.
[0036] In a second aspect, the present invention provides a gadolinium oxide doped cerium oxide nanocomposite material, wherein the gadolinium oxide doped cerium oxide nanocomposite material is prepared by the method for preparing the gadolinium oxide doped cerium oxide nanocomposite material according to the first aspect.
[0037] Preferably, the average particle size of the gadolinium oxide doped cerium oxide nanocomposite material is 5-100 nm, preferably 10-50 nm, for example, it can be 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc., so that it has a small particle size.
[0038] The present invention also provides a gadolinium oxide-doped cerium oxide ceramic and a preparation method thereof, the preparation method comprising the following steps:
[0039] The gadolinia-doped cerium oxide nanocomposite material according to the second aspect is subjected to uniaxial cold pressing at a pressure of 100-300 MPa, and then heated to 1450° C. at a heating rate of 5° C. / min and kept for 5 hours for sintering to obtain the gadolinia-doped cerium oxide ceramic, wherein the relative density of the ceramic is >97%.
[0040] In a third aspect, the present invention provides a solid oxide fuel cell, comprising the gadolinium oxide-doped cerium oxide nanocomposite material according to the second aspect.
[0041] The gadolinium oxide-doped cerium oxide nanocomposite material provided by the present invention can be applied to anode, cathode or electrolyte materials in solid oxide fuel cells, thereby achieving the technical effect of reducing costs and increasing efficiency.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] The present invention provides a method for preparing a gadolinium oxide doped cerium oxide nanocomposite material. The present invention uses dextran as a macromolecular biotemplate, which loses protons in a solution and provides negatively charged binding sites, thereby being able to chelate metal cations. Compared with small molecule chelating agents, the long-chain macromolecular biotemplate provided by the present invention can maintain a good dispersion effect on metal cations, avoiding agglomeration between subsequently formed nanoparticles, and at the same time, the long-chain macromolecular biotemplate can help guide and regulate crystal growth, and finally obtain a powder with a small particle size and a high specific surface area. In addition, the present invention removes the dextran chelating agent through a secondary calcination process, so as to obtain a high-purity gadolinium oxide doped cerium oxide nanocomposite powder material.
[0044] The preparation method provided by the present invention has the advantages of simple operation, low cost, environmental friendliness and short preparation time, and the preparation method has high repeatability and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The X-ray diffraction patterns of the gadolinium oxide-doped cerium oxide nanocomposites prepared in Examples 2 and 9-11 of the present invention;
[0046] Figure 2 The SEM microscopic morphology of the gadolinium oxide doped cerium oxide nanocomposite material prepared in Example 2 and Examples 9-11 of the present invention;
[0047] Figure 3 The SEM microscopic morphology of the surface and cross section of the gadolinium oxide doped cerium oxide ceramic electrolyte prepared in Example 11 of the present invention;
[0048] Figure 4 This is an EDS spectrum analysis diagram of the surface of the gadolinium oxide doped cerium oxide ceramic electrolyte prepared in Example 11 of the present invention;
[0049] Figure 5 These are SEM microscopic morphology images of the gadolinium oxide-doped cerium oxide nanocomposite materials prepared in Example 1 (left figure) and Comparative Example 4 (right figure) of the present invention. DETAILED DESCRIPTION
[0050] The technical solution of the present invention is further described below by combining the accompanying drawings and specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0051] The dextran chelating agent used in the examples and comparative examples of the present invention is Dextran dextran purchased from Shanghai MacLean Biochemical Technology Co., Ltd., with a molecular weight of 70,000.
[0052] Example 1
[0053] This embodiment provides a gadolinium oxide doped cerium oxide nanocomposite material and a preparation method thereof. The chemical formula of the gadolinium oxide doped cerium oxide nanocomposite material is Ce 0.9 G 0.1 O 1.95 , which comprises the following steps:
[0054] (1) According to the molar ratio of cerium ion to gadolinium ion of 9:1, cerium acetate sesquihydrate [Ce(CH3COO)3·3 / 2H2O] and gadolinium acetate tetrahydrate [Gd(CH3COO)3·4H2O] were weighed, and the weighed cerium acetate sesquihydrate and gadolinium acetate tetrahydrate were dissolved in deionized water, and stirred at 400 r / min at room temperature for 1.5 h to obtain a mixed salt solution, wherein the total concentration of metal ions in the mixed salt solution was 0.1 mol / L.
[0055] (2) According to the mass ratio of the total mass of cerium acetate sesquihydrate and gadolinium acetate tetrahydrate to the mass ratio of the dextran chelating agent being 10:1, the dextran chelating agent was weighed and added to the mixed salt solution in step (1), and stirred at 400 r / min for 1.5 h to obtain a reaction solution.
[0056] (3) Turn on the electric heating plate for heating, heat the reaction solution of step (2) to 80°C for complexation reaction, stir at 400 r / min until a gel or solid is obtained, dry the gel or solid in a constant temperature drying oven at 70°C for 12 h to obtain a hard solid, and ball mill it to obtain a precursor material.
[0057] (4) placing the precursor material obtained in step (3) in a tube furnace for a first calcination treatment at 400° C. for 4 h, with a heating rate of 3° C. / min for the first calcination treatment; after the product of the first calcination treatment is naturally cooled, grinding is performed and a second calcination treatment is performed at 400° C. for 2 h, with a heating rate of 5° C. / min for the second calcination treatment, to obtain a product with the chemical formula Ce 0.9 G 0.1 O 1.95 The material is denoted as GDC10.
[0058] Example 2
[0059] The difference between this embodiment and embodiment 1 is that in step (1), cerium acetate sesquihydrate [Ce(CH3COO)3·3 / 2H2O] and gadolinium acetate tetrahydrate [Gd(CH3COO)3·4H2O] are weighed in a molar ratio of cerium ions to gadolinium ions of 4:1 to obtain a mixture having a chemical formula of Ce 0.8 G 0.2 O 1.90 The material is denoted as GDC20, and the rest is the same as that in Example 1.
[0060] Example 3
[0061] The difference between this embodiment and embodiment 1 is that in step (1), cerium acetate sesquihydrate [Ce(CH3COO)3·3 / 2H2O] and gadolinium acetate tetrahydrate [Gd(CH3COO)3·4H2O] are weighed in a molar ratio of cerium ions to gadolinium ions of 7:3 to obtain a mixture having a chemical formula of Ce 0.7 G 0.3 O 1.85 The material is denoted as GDC30, and the rest is the same as that in Example 1.
[0062] Example 4
[0063] The difference between this embodiment and embodiment 1 is that in step (3), the gel or solid is dried in a constant temperature drying oven at 100° C. for 6 h to obtain a hard solid, which is then ball-milled to obtain a precursor material. The rest is the same as embodiment 1.
[0064] Example 5
[0065] The difference between this embodiment and embodiment 1 is that in step (1), cerium nitrate hexahydrate [Ce(NO)3·6H2O] and gadolinium nitrate hexahydrate [Gd(NO)3·6H2O] are weighed in a molar ratio of cerium ion to gadolinium ion of 9:1, and the rest is the same as embodiment 1.
[0066] Example 6
[0067] The difference between this embodiment and embodiment 1 is that in step (2), the dextran chelating agent is weighed in a ratio of 1:1 between the total mass of cerium acetate sesquihydrate and gadolinium acetate tetrahydrate and the mass of the dextran chelating agent, and the rest is the same as embodiment 1.
[0068] Example 7
[0069] The difference between this embodiment and embodiment 1 is that in step (2), the dextran chelating agent is weighed in a ratio of 20:1 between the total mass of cerium acetate sesquihydrate and gadolinium acetate tetrahydrate and the mass of the dextran chelating agent, and the rest is the same as embodiment 1.
[0070] Example 8
[0071] The difference between this embodiment and embodiment 1 is that the total concentration of metal ions in the mixed salt solution in step (1) is 0.5 mol / L, and Ce 0.9 G 0.1 O 1.95 The materials are the same as those in Example 1.
[0072] Example 9
[0073] The difference between this embodiment and embodiment 2 is that in step (4), the precursor material obtained in step (3) is placed in a tubular furnace for a first calcination treatment at 600°C for 4 hours, and the heating rate of the first calcination treatment is 3°C / min; after the product of the first calcination treatment is naturally cooled, it is ground and subjected to a second calcination treatment at 600°C for 2 hours, and the heating rate of the second calcination treatment is 3°C / min. The rest is the same as in embodiment 2.
[0074] Example 10
[0075] The difference between this embodiment and embodiment 2 is that in step (4), the precursor material obtained in step (3) is placed in a tubular furnace for a first calcination treatment at 800°C for 4 hours, and the heating rate of the first calcination treatment is 3°C / min; after the product of the first calcination treatment is naturally cooled, it is ground and subjected to a second calcination treatment at 800°C for 2 hours, and the heating rate of the second calcination treatment is 3°C / min. The rest is the same as in embodiment 2.
[0076] Embodiment 11
[0077] The difference between this embodiment and embodiment 2 is that in step (4), the precursor material obtained in step (3) is placed in a tubular furnace for a first calcination treatment at 900°C for 4 hours, and the heating rate of the first calcination treatment is 3°C / min; after the product of the first calcination treatment is naturally cooled, it is ground and subjected to a second calcination treatment at 900°C for 2 hours, and the heating rate of the second calcination treatment is 3°C / min. The rest is the same as in embodiment 2.
[0078] Example 12
[0079] The difference between this embodiment and embodiment 2 is that in step (2), the mass ratio of the total mass of cerium acetate sesquihydrate and gadolinium acetate tetrahydrate to the mass ratio of dextran chelating agent is 105:1, and the rest is the same as embodiment 2.
[0080] Comparative Example 1
[0081] The difference between this comparative example and Example 1 is that in step (4), the precursor material obtained in step (3) is placed in a tube furnace for calcination at 400° C. for 4 h, and the calcined product is naturally cooled and then ground to obtain Ce 0.9 G 0.1 O 1.95 Materials and other details are the same as those in Example 1.
[0082] Comparative Example 2
[0083] The difference between this comparative example and Example 1 is that in step (4), the precursor material obtained in step (3) is placed in a tube furnace for calcination at 600° C. for 4 h, and the calcined product is naturally cooled and then ground to obtain Ce 0.9 G 0.1 O 1.95 Materials and other details are the same as those in Example 1.
[0084] Comparative Example 3
[0085] The difference between this comparative example and Example 1 is that in step (4), the precursor material obtained in step (3) is placed in a tube furnace for calcination at 800° C. for 4 h, and the calcined product is naturally cooled and then ground to obtain Ce 0.9 G 0.1 O 1.95 Materials and other details are the same as those in Example 1.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 1 is that the dextran chelating agent is replaced with an equal amount of sucrose, and the rest is the same as Example 1.
[0088] Test conditions
[0089] The gadolinium oxide doped cerium oxide nanocomposites provided in Examples 1 to 12 and Comparative Examples 1 to 4 were tested, and the testing method was as follows:
[0090] XRD and SEM were used to perform phase analysis and micromorphology analysis on the products in the above-mentioned embodiments and comparative examples. In addition, the present invention calculated the grain size of the products in Example 2 and Examples 9-11 by using the Scherrer formula (D=Kλ / (βcosθ)), where D is the grain size, K is a constant, λ is the wavelength of the X-ray, β is the half-height width of the diffraction peak, and θ is the diffraction angle. The specific surface area of the products in Example 2 and Examples 9-11 was characterized by nitrogen adsorption. The carbon residue of the products in Example 2 and Examples 9-11 was characterized by a carbon-sulfur analyzer.
[0091] The gadolinia-doped cerium oxide ceramics were prepared using the gadolinia-doped cerium oxide nanocomposites in Example 2 and Examples 9-11. The preparation method was as follows: the gadolinia-doped cerium oxide nanocomposites in Example 2 were uniaxially cold pressed at a pressure of 230 MPa, then placed in a muffle furnace and heated to 1450° C. at a rate of 5° C. / min and kept warm for 5 h, then cooled to room temperature with the furnace to obtain gadolinia-doped cerium oxide ceramics.
[0092] The density of the gadolinium oxide doped cerium oxide ceramics was calculated by the Archimedean drainage method, and the surface and cross-section of the gadolinium oxide doped cerium oxide ceramics were microscopically analyzed by SEM.
[0093] The test results are shown in Table 1:
[0094] Table 1
[0095]
[0096] As can be seen from Table 1, as the calcination temperature increases, the grain size of the gadolinium oxide doped cerium oxide nanocomposite material increases, the specific surface area continues to decrease, and the carbon residue decreases, making the powder purer, resulting in an increase in its relative density, that is, all gadolinium oxide doped cerium oxide ceramic blocks have obtained a high relative density of >97%. However, a large amount of carbon residue will cause defects in the gadolinium oxide doped cerium oxide ceramic during the sintering process, and will affect the electrochemical performance of the gadolinium oxide doped cerium oxide nanocomposite material as a solid oxide fuel cell component. As the carbon residue further decreases, its sintering density increases slightly, until the carbon residue of the sintering temperature 800°C and 900°C treatment example is <0.1wt%, and its relative density is almost unchanged. Moreover, as the carbon residue decreases, the electrochemical performance of the gadolinium oxide doped cerium oxide nanocomposite material will be further improved. In order to further reduce the carbon residue in the product and obtain a high-purity product, the calcination temperature is preferably >600°C. The preparation method provided by the present invention has the advantages of short preparation time, and the gadolinium oxide-doped cerium oxide nanocomposite material prepared by this method has small particle size and high sintering activity, so that it can achieve high sintering density, which is a prerequisite for the operation of solid oxide fuel cell electrolyte materials.
[0097] from Figure 1 It can be seen that the X-ray diffraction patterns of the gadolinium oxide doped cerium oxide nanocomposites prepared in Examples 2 and 9-11 of the present invention are perfectly consistent with the standard card JCPDS: 75-0162, and no impurity peaks appear, which confirms that the gadolinium oxide doped cerium oxide nanocomposites have the characteristics of high purity.
[0098] from Figure 2 It can be seen that the gadolinium oxide-doped cerium oxide nanocomposites prepared in Example 2 and Examples 9-11 of the present invention are spherical in shape and have a small particle size.
[0099] from Figure 3-4 It can be seen that the elements in the gadolinium oxide-doped cerium oxide ceramic electrolyte prepared in Example 11 of the present invention are evenly distributed, and the block is dense.
[0100] Comparing Example 1 and Comparative Example 4, it can be seen that Figure 5It can be seen that when small molecule sugar (such as sucrose) is used as a biological template, due to its small molecular weight, there is no macromolecular long chain structure, and it is impossible to maintain the uniform dispersion of metal cations, resulting in irregular aggregation with a size of >10μm. However, the long chain structure of macromolecular polysaccharides (dextran) can maintain ion dispersion in space, thus presenting light aggregation of hundreds of nanometers to several microns, and the aggregation shape is spherical, which will improve the sintering activity of gadolinium oxide doped cerium oxide nanocomposites.
[0101] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a gadolinium oxide-doped cerium oxide nanocomposite material, characterized in that: The method comprises the following steps: A mixed salt solution containing a gadolinium source and a cerium source is subjected to a complexation reaction with a dextran chelating agent to obtain a precursor material; the precursor material is subjected to a secondary calcination treatment to obtain a gadolinium oxide-doped cerium oxide nanocomposite material.
2. The method according to claim 1, characterized in that The gadolinium source includes any one of hydrated gadolinium nitrate, hydrated gadolinium acetate or gadolinium acetylacetonate or a combination of at least two thereof, preferably hydrated gadolinium acetate; Preferably, the cerium source includes any one of hydrated cerium nitrate, hydrated cerium acetate, hydrated cerium carbonate, cerium ammonium nitrate or cerium acetylacetonate, or a combination of at least two thereof, preferably hydrated cerium acetate.
3. The method according to claim 1 or 2, characterized in that: The molar ratio of cerium ions in the cerium source to gadolinium ions in the gadolinium source is (2-15):1, preferably (4-9):1; Preferably, the total concentration of metal ions in the mixed salt solution is 0.05-5 mol / L, preferably 0.1-1 mol / L.
4. The method according to any one of claims 1 to 3, characterized in that The mass ratio of the total mass of the gadolinium source and the cerium source to the dextran chelating agent is (0.1-100):1, preferably (1-20):
1.
5. The method according to any one of claims 1 to 4, characterized in that The complex reaction is carried out under stirring; Preferably, the stirring rate is 30-1000r / min, preferably 300-500r / min; Preferably, the stirring time is 0.5-24 h, preferably 1.5 h.
6. The method according to any one of claims 1 to 5, characterized in that The temperature of the complexation reaction is 60-100°C, preferably 70-90°C; Preferably, after the complex reaction is completed, drying and grinding treatments are sequentially included; Preferably, the drying temperature is 20-180°C, preferably 70-100°C; Preferably, the drying time is 2-72 hours, preferably 6-14 hours.
7. The method according to any one of claims 1 to 6, characterized in that The secondary calcination treatment includes a first calcination treatment and a second calcination treatment in sequence; Preferably, the temperature of the first calcination treatment and the second calcination treatment is independently 300-1200° C., preferably 600-900° C.; Preferably, the heating rates of the first calcination treatment and the second calcination treatment are independently 0.5-10°C / min, preferably 3-5°C / min; Preferably, the time of the first calcination treatment and the second calcination treatment are each independently 0.5-24 hours, preferably 2-6 hours.
8. A gadolinium oxide-doped cerium oxide nanocomposite material, characterized in that: The gadolinium oxide doped cerium oxide nanocomposite material is prepared by the method for preparing the gadolinium oxide doped cerium oxide nanocomposite material according to any one of claims 1 to 7.
9. The gadolinium oxide-doped cerium oxide nanocomposite material according to claim 8, characterized in that: The average particle size of the gadolinium oxide doped cerium oxide nanocomposite material is 5-100 nm, preferably 10-50 nm.
10. A solid oxide fuel cell, characterized in that: The solid oxide fuel cell comprises the gadolinium oxide-doped cerium oxide nanocomposite material according to claim 8 or 9.